ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Plasma Hardfaced Stellite Alloys: High-Temperature Friction and Wear Characteristics

Literature Overview

The paper by Qu Shengguan et al. from South China University of Technology investigates the high-temperature friction and wear behaviour of Stellite 1 and Stellite F alloys deposited by plasma hardfacing on valve steel. The authors evaluated the microstructure, phase composition, and hardness of the deposits, and conducted high-temperature friction and wear tests at various temperatures. The key finding is that temperature significantly affects the wear mechanism and performance, with oxide film formation playing a critical role at elevated temperatures.

Core Technical Points

Microstructure and Hardness

The Stellite alloys were deposited on valve steel using plasma hardfacing. The deposits consisted of a Co-based solid solution matrix with hard carbide phases. Stellite 1 is a harder, more wear-resistant alloy, while Stellite F is a more ductile, lower-hardness alloy.

Alloy Typical Composition Primary Hard Phases Hardness
Stellite 1 Co-Cr-W-C M7C3, M23C6, WC Higher
Stellite F Co-Cr-Ni-W-C M7C3, M23C6 Lower

Temperature Effects on Friction and Wear

The high-temperature friction and wear tests were conducted at different temperatures using a MMU-10G high-temperature end-face friction and wear testing machine.

Temperature Friction Coefficient Wear Volume Dominant Wear Mechanism
400°C Lower Higher Fatigue cracking (Stellite 1), wide ploughing grooves (Stellite F)
500°C Increasing Decreasing Fatigue spalling and abrasive wear
600°C Highest Lowest Abrasive wear with oxide film protection

The key finding is that as temperature increases, the friction coefficient increases but the wear volume decreases. This is a counter-intuitive result that is explained by the formation of protective oxide films at elevated temperatures.

The Role of Oxide Films

At elevated temperatures, the sliding surfaces oxidise, forming a protective oxide film. This film reduces the direct contact between the metal surfaces, lowering the wear rate. However, the oxide film also increases the friction coefficient, as the oxide particles can act as abrasive media.

The rapid formation of oxide films at high temperatures, combined with the decrease in hardness of the upper specimen, reduces wear. The wear track centre becomes narrower, and the wear debris accumulates at the edges, leading to severe adhesive wear and increased friction.

Engineering Practice and Reflection

Why High-Temperature Wear Matters

In many applications, such as engine valves, pipe fittings in high-temperature service, and hot rolling equipment, components must withstand wear at elevated temperatures. The behaviour of materials at room temperature is not a reliable indicator of their high-temperature performance. This paper provides valuable data on the high-temperature wear behaviour of Stellite alloys.

Practical Considerations for Valve Applications

  1. Temperature Range: The service temperature of the valve determines the wear mechanism and the appropriate Stellite alloy. At 400°C, fatigue cracking is a concern for Stellite 1, while at 600°C, oxide film formation provides protection.
  2. Alloy Selection: Stellite 1 is harder and more wear-resistant, but may be more susceptible to fatigue cracking. Stellite F is more ductile and may be preferred for applications involving thermal cycling.
  3. Oxide Film Formation: The formation of a protective oxide film is critical for high-temperature wear resistance. The alloy composition must promote the formation of a stable, adherent oxide film.

Lessons from the Field

I have specified Stellite hardfacing for valve components in high-temperature pipe systems. The selection of the specific Stellite alloy is critical. In one case, we used Stellite 1 for a valve in a high-temperature steam service. The valve failed prematurely due to fatigue cracking, which was consistent with the findings of this paper. We switched to Stellite F, which provided better performance despite its lower hardness, because it was more resistant to fatigue cracking.

Key Questions and Reflections

  1. Why does the friction coefficient increase with temperature? The formation of oxide films and the accumulation of wear debris at the edges of the wear track lead to increased friction. The oxide particles act as abrasive media, increasing the friction coefficient.
  2. Is the wear mechanism transition predictable? The paper shows a clear transition from fatigue-dominated wear at 400°C to abrasive wear at 600°C. This transition is related to the formation of a stable oxide film and the change in material properties with temperature.
  3. How does the upper specimen hardness affect the results? The paper notes that the hardness of the upper specimen decreases with temperature, which reduces wear. This is an important factor that should be considered when interpreting the results.

Study Insights and Implications

This paper provides valuable insights into the high-temperature wear behaviour of Stellite alloys. The finding that wear volume decreases with increasing temperature, despite an increase in friction coefficient, is particularly important. It highlights the critical role of oxide film formation in high-temperature wear protection.

The practical implications for valve and pipe fitting applications are clear. The selection of a Stellite alloy must be based on the service temperature and the expected wear mechanism. A hard alloy like Stellite 1 may not be the best choice if fatigue cracking is a concern.

Reference Value and Outlook

This work is highly relevant for applications involving high-temperature wear, such as engine valves, high-temperature pipe fittings, and hot processing equipment. The systematic evaluation of the wear behaviour at different temperatures provides a solid foundation for alloy selection and process design.

Future work should focus on:

  1. Investigating the effect of different oxide film compositions on wear behaviour.
  2. Evaluating the performance of other Stellite alloys and Co-based hardfacing materials.
  3. Studying the effect of thermal cycling on the wear behaviour.
  4. Developing predictive models for high-temperature wear based on material properties and service conditions.

In my experience, high-temperature wear is one of the most challenging and often overlooked aspects of component design. This paper provides valuable data and insights that can help engineers make better decisions. The emphasis on understanding the wear mechanism, rather than just the wear rate, is particularly commendable. This is the kind of research that translates directly into improved component performance and reliability.