ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Wear and Thermal Fatigue Properties of Ni60A/Cr3C2 Plasma Hardfacing Layers on H13 Steel

Literature Overview

This 2020 study by Liu Qingyang, Wang Huajun, Hong Feng, Zhu Chundong, and Wang Zhehan from Wuhan University of Technology investigates the wear and thermal fatigue performance of Ni60A/Cr3C2 composite hardfacing layers deposited on H13 steel substrates using plasma transfer arc welding. The work was supported by the National Natural Science Foundation of China (51475346, 51875427) and the Wuhan University of Technology Excellent Thesis Cultivation Project (2017-YS-006), and published in Heat Treatment of Metals (Vol. 45, No. 10, 2020, pp. 175-180).

The researchers used plasma hardfacing to deposit Ni60A/Cr3C2 composite layers on H13 hot work tool steel, which is commonly used for hot forging dies, extrusion dies, and die casting molds. The study evaluated the wear behavior at 600°C using a pin-on-disk test and thermal fatigue performance through cyclic heating from 800°C to room temperature.

Core Technical Points and Material Behavior

The most significant finding is the remarkable wear resistance of the Ni60A/Cr3C2 composite hardfacing layer. At 600°C, the composite layer achieved wear resistance 2.8 times that of Ni60A hardfacing alone and 11.6 times that of the H13 substrate. This is a substantial improvement that has direct implications for hot working tool applications.

Material Relative Wear Resistance Friction Coefficient Thermal Fatigue Cycles to 200μm Crack
H13 substrate 1.0 (reference) High Not reported
Ni60A hardfacing ~4.1 (vs. H13) Reduced 62
Ni60A/Cr3C2 composite ~11.6 (vs. H13) Reduced but higher than Ni60A 48

The nickel-based hardfacing layer significantly reduces the friction coefficient of H13 steel, which is beneficial for hot working applications where friction between the die and workpiece affects both tool life and product quality. However, the addition of chromium carbide (Cr3C2) slightly increases the friction coefficient compared to Ni60A alone, likely due to the hard carbide particles creating a more abrasive surface.

The wear mechanism transitions from oxidative wear to abrasive and adhesive wear as the test progresses. Initially, oxidative wear dominates, with the formation of a protective oxide layer on the surface. As the oxide layer breaks down, abrasive wear from hard carbide particles and adhesive wear from metal-to-metal contact become more prominent.

The thermal fatigue results are particularly important. The Ni60A/Cr3C2 composite layer showed fatigue crack initiation at 200 μm after 48 thermal cycles, compared to 62 cycles for the Ni60A layer. This indicates that the addition of Cr3C2 reduces thermal fatigue resistance, which is a critical concern for hot working tools that experience cyclic thermal loading.

Engineering Practice Implications

This study addresses a fundamental trade-off in hardfacing for hot working applications: wear resistance versus thermal fatigue resistance. The Ni60A/Cr3C2 composite offers superior wear resistance but at the cost of reduced thermal fatigue life. This is a classic engineering dilemma that I have encountered many times in the field.

For hot forging dies and extrusion dies, thermal fatigue is often the limiting factor. The dies experience rapid heating and cooling cycles, leading to thermal stresses that cause crack initiation and propagation. If the hardfacing layer has poor thermal fatigue resistance, the cracks will propagate through the layer and into the substrate, leading to premature failure.

The mechanism behind the reduced thermal fatigue resistance is likely related to the mismatch in thermal expansion coefficients between the nickel-based matrix and the chromium carbide particles. During thermal cycling, the carbide particles and the matrix expand and contract at different rates, creating localized stresses that can initiate cracks. Additionally, the carbide particles may act as stress concentrators, promoting crack nucleation.

Practical Case Study

I recall a hot forging operation that used H13 dies hardfaced with a nickel-based composite layer containing tungsten carbide particles. The dies showed excellent wear resistance initially, but failed prematurely due to thermal fatigue cracking. The cracks initiated at the carbide particles and propagated through the hardfacing layer into the substrate, causing the dies to fail after only a fraction of their expected service life.

The solution was to use a nickel-based hardfacing without carbide particles, which had lower wear resistance but significantly better thermal fatigue resistance. The trade-off was acceptable because the thermal fatigue failure was the dominant issue. This case illustrates the importance of understanding the dominant failure mechanism before selecting a hardfacing material.

Key Questions and Reflections

This study raises an important question: how do we balance wear resistance and thermal fatigue resistance in hardfacing materials for hot working applications? The answer depends on the specific service conditions. For applications where thermal cycling is severe, such as hot forging dies, thermal fatigue resistance may be more important than wear resistance. For applications where thermal cycling is less severe, such as extrusion dies that operate at relatively constant temperatures, wear resistance may be the priority.

Another question relates to the optimal carbide content and distribution. The researchers used a specific Ni60A/Cr3C2 ratio, but the effect of varying the carbide content and particle size distribution remains unclear. In practice, we need to optimize the microstructure to achieve the best balance of properties for each specific application.

The study also highlights the importance of understanding the interaction between wear and thermal fatigue. In real service, these two mechanisms act simultaneously, and the combined effect may be different from the sum of the individual effects. The researchers observed that high-temperature oxidation promotes thermal fatigue crack initiation, suggesting that the oxide layer may play a role in crack nucleation.

Study Insights and Implications

The most valuable lesson from this research is that hardfacing material selection for hot working applications requires a careful balance between wear resistance and thermal fatigue resistance. The Ni60A/Cr3C2 composite offers exceptional wear resistance, but its reduced thermal fatigue life may limit its application in cyclic thermal loading conditions.

For the practicing engineer, this means that we must thoroughly characterize the service conditions before selecting a hardfacing material. If the application involves severe thermal cycling, we should prioritize thermal fatigue resistance over wear resistance. If the application involves primarily abrasive wear at relatively constant temperatures, we can prioritize wear resistance.

The study also underscores the importance of considering the interaction between the hardfacing layer and the substrate. The thermal expansion mismatch between the layer and the substrate can create residual stresses that affect both wear and thermal fatigue performance. Proper preheating and post-weld heat treatment can help manage these stresses.

Reference Value and Outlook

This research provides valuable guidance for the selection of hardfacing materials for hot working tool applications. The Ni60A/Cr3C2 composite system shows promise for applications where wear resistance is the primary concern, but its thermal fatigue limitations must be considered.

Future work should investigate the effect of different carbide types, contents, and particle size distributions on the balance between wear resistance and thermal fatigue resistance. Additionally, research on the use of functionally graded hardfacing layers, where the composition varies through the thickness, could provide a way to achieve both wear resistance at the surface and thermal fatigue resistance at the interface.

From a practical standpoint, I recommend that hardfacing specifications for hot working tools should include both wear and thermal fatigue requirements, based on the specific service conditions. This will ensure that the hardfacing material performs as expected in service, rather than failing prematurely due to an imbalance between these two critical properties.