Microstructure and Properties of Stainless Steel Surfacing on Q235 Steel
Literature Overview and Core Findings
This paper by Wu Zhisheng, Yun Hui, Liu Cuirong, Li Ke and Quan Wanglin from Taiyuan University of Science and Technology, published in Welding Technology in 2014, investigates the microstructure and hardness of 3Cr13 stainless steel hardfacing layers deposited on Q235 steel plates using submerged arc welding (SAW). The study addresses a common industrial problem: how to achieve a wear-resistant stainless steel layer on low-cost carbon steel substrates.
The key finding is that when the number of hardfacing layers reaches three, the hardness of the hardfacing alloy is essentially unaffected by base metal dilution. The average surface hardness of the hardfacing layer is HRC 45.9, and the microstructure consists of acicular martensite plus retained austenite.
Technical Interpretation and Metallurgical Analysis
Dilution Control in Multi-Layer Hardfacing
The most important practical aspect of this paper is the dilution control. When the first layer of hardfacing is deposited, the base metal dilution can be as high as 30-40%, which significantly reduces the alloy content in the deposit. This is why the first layer often fails to achieve the desired hardness and corrosion resistance.
| Layer Number | Dilution Rate (%) | Alloy Content (%Cr) | Expected Hardness (HRC) | Microstructure |
|---|---|---|---|---|
| 1 | 30-40 | 8-10 | 25-30 | Ferrite + Pearlite + Martensite |
| 2 | 15-25 | 12-14 | 35-40 | Martensite + Retained Austenite |
| 3 | 5-10 | 14-16 | 45-48 | Acicular Martensite + Retained Austenite |
The paper confirms that by the third layer, the dilution effect is negligible, and the deposit achieves its full alloy composition and hardness. This is a critical practical point because it means that for most applications, a minimum of three layers is required to achieve the desired properties.
Hardness and Microstructure Relationship
The average hardness of HRC 45.9 is consistent with a martensitic microstructure containing retained austenite. The acicular martensite provides high hardness and wear resistance, while the retained austenite contributes to toughness and prevents brittle fracture.
The presence of retained austenite is particularly important in wear applications because it can transform to martensite under service loading, providing a work-hardening effect similar to that described in the CrMnB alloy paper. This is a common design feature in wear-resistant hardfacing alloys.
Integration with Engineering Practice
Application in Wear-Resistant Components
The combination of Q235 substrate with 3Cr13 hardfacing is widely used in applications such as:
- Chute liners and hopper liners in mining and cement plants
- Crusher rolls and hammers
- Bucket teeth and cutting edges for earthmoving equipment
- Guide vanes and wear plates in material handling systems
The economic advantage is significant: Q235 steel costs approximately $500-600 per tonne, while 3Cr13 stainless steel costs approximately $2,500-3,000 per tonne. By using Q235 as the substrate and applying a 3-5 mm hardfacing layer, the material cost is reduced by 60-70% while achieving comparable wear resistance.
Welding Process Parameters
For SAW hardfacing of 3Cr13 on Q235, the typical parameters are:
- Welding current: 300-400 A
- Arc voltage: 28-32 V
- Welding speed: 25-35 cm/min
- Preheat temperature: 100-150°C
- Interpass temperature: 200-250°C
- Flux type: agglomerated flux with basicity index of 1.5-2.0
The preheat is necessary to prevent hydrogen-induced cracking in the martensitic deposit. The interpass temperature must be controlled to avoid excessive grain growth and to ensure proper transformation of austenite to martensite.
Common Defects and Countermeasures
| Defect | Root Cause | Countermeasure |
|---|---|---|
| Cracking | High hardness, hydrogen, restraint | Preheat, low-hydrogen flux, controlled interpass temperature |
| Porosity | Moisture in flux, surface contamination | Drying flux at 300-350°C for 2 hours, cleaning surface |
| Undercut | Excessive current or speed | Reduce current, adjust welding speed |
| Dilution non-uniformity | Inconsistent process parameters | Use automated welding, monitor parameters |
Key Questions and Reflections
The paper does not address the corrosion resistance of the hardfacing layer, which is an important consideration in many applications. While 3Cr13 is a martensitic stainless steel with moderate corrosion resistance, the hardfacing layer may not provide adequate corrosion protection in aggressive environments.
In my experience, for applications requiring both wear resistance and corrosion resistance, it is often better to use duplex stainless steel or nickel-based alloy hardfacing, despite the higher material cost. The choice depends on the specific service conditions and the expected service life.
Another important consideration is the post-weld heat treatment. The paper does not mention whether PWHT is required after hardfacing. In practice, if the component is thick or highly restrained, PWHT at 550-600°C for 2-4 hours may be necessary to relieve residual stresses and prevent stress corrosion cracking.
Study Insights and Practical Implications
This paper provides valuable practical information for engineers involved in hardfacing of carbon steel components. The confirmation that three layers are sufficient to achieve full alloy composition and hardness is a key takeaway that can guide process design.
For the practicing engineer, the key lessons are:
- A minimum of three hardfacing layers is required to overcome base metal dilution
- The hardness of the third layer is essentially independent of dilution and reaches HRC 45-48
- Preheating and interpass temperature control are essential to prevent cracking
- The microstructure of acicular martensite plus retained austenite provides an optimal combination of hardness and toughness
In conclusion, this paper demonstrates that SAW hardfacing of 3Cr13 on Q235 is a practical and economical solution for wear-resistant components. The key to success is proper control of dilution through multi-layer deposition and careful management of welding parameters to prevent defects. For engineers involved in the design and fabrication of wear-resistant equipment, this paper provides a solid technical foundation for process development.
Zhuojin Pipe Fitting Co., Ltd