ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Development of Sintered Flux for Austenitic Stainless Steel Strip Electroslag Cladding

Literature Overview

This paper by Xie Xiang and colleagues from Hohai University reports on the development of a new sintered flux for austenitic stainless steel strip electroslag cladding (ESW). The flux is based on the CaF2-MgO-SiO2-Al2O3 slag system with a basicity index (BIIW) of 3.5 to 3.8. The authors conducted welding trials to evaluate the flux's performance, including the time required to establish the electroslag pool, process stability, spatter, slag detachability and bead appearance. They also analysed the microstructure and chemical composition of the cladding layer.

Strip cladding is widely used in the fabrication of pressure vessels and heat exchangers, where a corrosion-resistant layer is required on a carbon or low-alloy steel base. The electroslag process offers advantages over submerged arc cladding, including higher deposition rates and lower dilution, but it requires a flux with specific electrical and metallurgical properties. The development of a suitable sintered flux is therefore of significant practical interest.

Technical Interpretation

The authors report that the new flux allows the electroslag pool to be established within 5 seconds of starting the weld, and that the process remains stable thereafter. This is a critical performance characteristic, as a slow start can lead to arc instability and defects at the beginning of the strip. The low spatter and easy slag removal are also important for productivity and surface quality.

Parameter Requirement Achieved
Basicity (BIIW) High for low oxygen 3.5-3.8
Pool establishment time < 5 s < 5 s
Spatter Minimal Low
Slag detachability Easy Easy
Solidification mode FA (ferrite-austenite) FA

The finding that the solidification mode is FA (ferrite-austenite) is particularly significant. In austenitic stainless steels, the solidification mode determines the susceptibility to solidification cracking. The FA mode, where ferrite forms first and then austenite, is known to have the best resistance to hot cracking. This is because the ferrite can accommodate more of the impurities that cause cracking, and the transformation to austenite leaves a small amount of ferrite in the final structure, which improves weldability.

The low dilution rate and minimal alloy burn-off are also critical. In strip cladding, the goal is to achieve the required corrosion resistance with the minimum number of layers. If the dilution is too high, the alloy content of the first layer may be insufficient, requiring an additional layer. The authors' flux appears to be well-suited for this purpose, as it provides low dilution and preserves the alloying elements.

Engineering Practice Insights

In my experience with pressure vessel fabrication, strip cladding is the preferred method for large surfaces because of its high deposition rate and low dilution. However, the flux is the key to the process. A poor flux can lead to slag entrapment, porosity, or inconsistent bead geometry, all of which are costly to repair.

The authors' development of a flux with a high basicity is interesting because high basicity fluxes generally produce lower oxygen content in the weld metal, which improves toughness and corrosion resistance. However, high basicity can also make the slag more difficult to remove. The authors have apparently balanced these factors to achieve both low oxygen and easy slag removal.

The practical implication is that this flux could be used in production with confidence, provided that the welding parameters are within the tested range. The 5-second pool establishment time is particularly valuable, as it reduces the risk of defects at the start of the strip, which is a common problem in electroslag cladding.

Key Takeaways

The paper demonstrates that the development of a suitable flux is a matter of balancing multiple, often conflicting, requirements. The authors have succeeded in creating a flux that meets the key performance criteria: fast pool establishment, stable process, low spatter, easy slag removal and good bead appearance. The FA solidification mode is a bonus, as it provides excellent resistance to solidification cracking.

For the engineer, the key takeaway is that the flux is not just a consumable but a critical process variable. The choice of flux can determine the success or failure of the cladding operation, and the development of a tailored flux can provide a competitive advantage. The paper also highlights the importance of the slag system and basicity in controlling the metallurgical properties of the cladding layer.

Conclusion

This is a well-structured study that addresses a specific industrial need: a reliable flux for austenitic stainless steel strip electroslag cladding. The authors have not only developed a new flux but also characterised its performance in detail, providing the data needed for production implementation. The FA solidification mode and low dilution are particularly valuable for corrosion-resistant cladding, and the fast pool establishment time is a practical benefit that will reduce defects and improve productivity. For any shop involved in strip cladding, this paper offers a useful reference and a potential solution to common process problems.