ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Shielding Gas Effects on (Nb,Ti)C Reinforced Iron-Based Composite Surfacing Layer

Why This Study Matters on the Shop Floor

Wear-resistant surfacing is a critical technology for components that operate in abrasive, erosive, or adhesive wear conditions. The conventional approach is to use hardfacing alloys such as chromium carbide, tungsten carbide, or vanadium carbide. However, these alloys are expensive and often difficult to apply. A more recent approach is to use composite surfacing layers reinforced with niobium and titanium carbides, which are formed in situ during the welding process. This paper by Zeng Bangxing and colleagues at Guangdong University of Technology and the Guangdong Provincial Key Laboratory of Modern Welding Technology examines the effect of shielding gas composition on the microstructure, hardness, and wear resistance of (Nb,Ti)C reinforced iron-based composite surfacing layers. The authors used three different shielding gases: pure Ar, 80%Ar+20%CO2, and pure CO2.

Why Shielding Gas Matters

The shielding gas in gas-shielded welding serves two primary functions:

  1. Protecting the weld pool from atmospheric contamination (oxygen, nitrogen, hydrogen).
  2. Influencing the arc characteristics, heat input, and weld pool chemistry.

For composite surfacing layers, the shielding gas also influences the formation and growth of carbide particles. Oxygen in the shielding gas can oxidize the carbide-forming elements (Nb, Ti), reducing the amount of carbide that forms. This is a critical factor that is often overlooked in surfacing applications.

Test Design and Results

The authors used gas-shielded welding to deposit (Nb,Ti)C reinforced iron-based composite surfacing layers using three different shielding gas compositions. The surfacing layers were analyzed for microstructure, carbide precipitation, microhardness, and wear resistance.

Parameter Pure Ar 80%Ar+20%CO2 Pure CO2
(Nb,Ti)C precipitation density 0.54 particles/μm² Intermediate 0.44 particles/μm²
Microhardness 708.2 HV Intermediate 620.3 HV
Wear loss 0.8 mg Intermediate 8.4 mg
Relative wear resistance Best (100%) Intermediate Worst (9.5% of pure Ar)
Oxygen content in deposit Lowest Intermediate Highest
Dominant wear mechanism Adhesive + fatigue + abrasive Adhesive + fatigue + abrasive Severe adhesive wear

The results show a clear trend: as the CO2 content in the shielding gas increases, the (Nb,Ti)C precipitation density decreases, the microhardness decreases, and the wear resistance decreases. The pure Ar shielding gas produces the best results, while pure CO2 produces the worst.

Microstructure and Wear Mechanisms

The authors analyzed the microstructure of the surfacing layers and identified the wear mechanisms. The (Nb,Ti)C particles are dispersed in a martensitic matrix. The carbide particles provide hardness and wear resistance, while the martensitic matrix provides toughness and support.

Effect of CO2 on Carbide Precipitation

The presence of CO2 in the shielding gas introduces oxygen into the weld pool. The oxygen reacts with niobium and titanium to form oxides, which reduces the amount of these elements available for carbide formation. The result is a lower density of (Nb,Ti)C particles in the deposit.

The authors found that pure CO2 shielding gas produces the lowest carbide density (0.44 particles/μm²), while pure Ar produces the highest (0.54 particles/μm²). This is a significant difference, and it directly correlates with the observed differences in hardness and wear resistance.

Wear Mechanisms

The wear mechanisms observed in the study are adhesive wear, fatigue wear, and abrasive wear. The pure Ar deposit exhibits the best wear resistance, with the wear mechanism being a combination of adhesive, fatigue, and abrasive wear. The pure CO2 deposit exhibits severe adhesive wear, which is the most damaging wear mechanism because it involves material transfer between the wearing surfaces.

The authors attribute the severe adhesive wear in the pure CO2 deposit to the lower hardness and the lower density of carbide particles. The softer surface is more susceptible to adhesive wear because the contact area between the surfaces is larger.

Practical Selection Criteria

This study provides clear guidance for selecting the shielding gas for (Nb,Ti)C reinforced composite surfacing. The practical implications are:

  1. Use pure Ar shielding gas for maximum carbide precipitation, hardness, and wear resistance.
  2. Avoid CO2-containing shielding gases if the application requires maximum wear resistance.
  3. If CO2 must be used for cost or operational reasons, expect a significant reduction in wear resistance.
  4. The shielding gas composition should be specified in the welding procedure specification (WPS) and verified during production.
Application Recommended Shielding Gas Rationale
High wear resistance required Pure Ar Maximum carbide precipitation, highest hardness
Moderate wear resistance, cost-sensitive 80%Ar+20%CO2 Acceptable performance, lower cost
General purpose, non-critical Pure CO2 Lowest cost, but significantly reduced performance

Shop Floor Implications

This study has direct implications for the shop floor. I have seen cases where a welding procedure was specified with a particular shielding gas, but the shop floor used a different gas because the specified gas was not available or was too expensive. The result was a component that failed prematurely in service.

The lesson is clear: the shielding gas is a critical process parameter, not an incidental detail. If the welding procedure specifies pure Ar, you must use pure Ar. Substituting a CO2-containing gas may save money on the gas, but it will cost you in component life.

Another shop floor consideration is the effect of shielding gas on the welding process itself. Pure Ar produces a more stable arc and less spatter than CO2-containing gases. This can affect the quality of the deposit and the productivity of the welding operation.

Key Questions and Reflections

The study raises several questions that I would put to any welding engineer or surfacing specialist:

  1. What is the effect of shielding gas on the deposition rate and welding productivity?
  2. What is the effect of shielding gas on the dilution of the substrate into the deposit?
  3. What is the effect of shielding gas on the residual stress in the deposit?
  4. Is the effect of shielding gas consistent across different substrate materials?
  5. What is the cost-benefit analysis of using pure Ar versus CO2-containing gases?

Study Insights and Implications

The key insight from this study is that the shielding gas composition has a profound effect on the microstructure and properties of (Nb,Ti)C reinforced composite surfacing layers. The oxygen introduced by CO2 in the shielding gas reacts with the carbide-forming elements, reducing the amount of carbide that forms. This reduces the hardness and wear resistance of the deposit.

The study also highlights the importance of process control in surfacing applications. The shielding gas is not just a protective medium; it is a reactive component that influences the metallurgy of the deposit. This is a lesson that many welding engineers overlook.

Reference Value and Outlook

This paper is a valuable reference for any engineer involved in wear-resistant surfacing. The comparison between different shielding gases is particularly useful because it demonstrates that the shielding gas is a critical process parameter that must be specified and controlled. Future work should extend the study to include:

The bottom line is that the shielding gas is a critical process parameter in composite surfacing. If you want maximum wear resistance, use pure Ar. If you use CO2-containing gases, you will pay a significant penalty in performance. This study gives you the data to make an informed decision.