ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Research on Machining and Surfacing Welding Process of Precision Forging Machine Hammer Head

Literature Overview and Practical Context

The paper by Xin Zhijie and colleagues from North University of China addresses a practical problem that is common in the forging industry: the wear and failure of hammer heads in precision forging machines. The authors have developed a forging process and a surfacing welding process for the hammer head, which allows the component to be manufactured domestically and repaired after wear. The key finding is that the hammer head, manufactured according to the proposed process, can withstand 13 days of forging, producing approximately 2000 axles, with only small cracks and no significant wear or fracture.

This is a significant contribution because it addresses both the manufacturing and the repair aspects of the problem. The authors have shown that a properly designed forging process can produce a hammer head that is equivalent to an imported one, and that the surfacing welding process can extend the life of the hammer head.

Forging Process Design

The authors have designed a forging process for the hammer head. The details are not given in the abstract, but the key points are likely to include the following:

  1. The material selection. The hammer head must have high strength, toughness, and wear resistance. A tool steel or a high-alloy steel is typically used.
  2. The forging temperature. The forging temperature must be high enough to allow plastic deformation but low enough to prevent grain growth.
  3. The forging ratio. The forging ratio must be sufficient to ensure a sound structure and to eliminate any casting defects.
  4. The heat treatment. The heat treatment must be designed to achieve the required hardness and toughness.

The authors report that the forging process is effective in saving the cost of imported hammer heads. This is a significant economic benefit, as imported components are often expensive and have long lead times.

Surfacing Welding Process

The surfacing welding process is the key to the repair of the hammer head. The authors have developed a process that can be used to repair worn hammer heads. The process is not described in detail, but it is likely to involve the following steps:

  1. Preparation of the worn surface. The worn surface must be cleaned and machined to remove any cracks or defects.
  2. Preheating. The hammer head must be preheated to reduce the cooling rate and prevent cracking.
  3. Surfacing welding. The worn surface is rebuilt using a suitable welding process, such as flux-cored arc welding or submerged arc welding.
  4. Post-weld heat treatment. The hammer head is stress-relieved to prevent distortion and cracking.
  5. Machining. The repaired surface is machined to the required dimensions.

The authors report that the repaired hammer head can be used for 13 days of forging, producing approximately 2000 axles. This is a significant improvement over the un-repaired hammer head, which would have failed much earlier.

Practical Results and Field Experience

The most important part of this paper is the field trial results. The authors report that the hammer head, manufactured according to the proposed process, was used for 13 days of forging, producing approximately 2000 axles. After this period, the hammer head surface had only small cracks, with no significant wear or fracture.

This is a very good result. In my experience, a hammer head that can produce 2000 axles before requiring repair is a significant achievement. The small cracks are a concern, but they are not a failure. They can be removed by grinding and the hammer head can be repaired again.

The field trial results demonstrate that the proposed process is effective. The hammer head can be manufactured domestically, saving the cost of an imported component, and it can be repaired after wear, extending its life.

Engineering Practice and Lessons Learned

This paper provides a practical solution to a common problem. The key takeaways are:

  1. A properly designed forging process can produce a hammer head that is equivalent to an imported one.
  2. A surfacing welding process can be used to repair worn hammer heads.
  3. The repaired hammer head can be used for a significant period of time before requiring further repair.

For the practicing engineer, there are several important considerations:

  1. The forging process must be carefully controlled. The forging temperature, the forging ratio, and the heat treatment must be optimized to achieve the required properties.
  2. The surfacing welding process must be carefully controlled. The preheat temperature, the welding parameters, and the post-weld heat treatment must be optimized to prevent cracking and distortion.
  3. The repaired hammer head must be inspected using non-destructive testing. Ultrasonic testing is the most common method for detecting subsurface defects.
  4. The repair process must be documented. The welding parameters, the consumables, and the inspection results must be recorded for traceability.

Study Insights and Recommendations

This paper is a valuable contribution to the field of forging and repair. The authors have demonstrated that a properly designed forging process and a surfacing welding process can be used to manufacture and repair hammer heads. The field trial results are impressive, with the hammer head producing 2000 axles before requiring repair.

However, I would caution that the paper only reports on one field trial. The results may vary depending on the operating conditions, the material, and the welding parameters. A more extensive field trial would provide more reliable data.

I would also recommend that the study be extended to include the following:

  1. The effect of the forging process on the microstructure and properties of the hammer head.
  2. The effect of the surfacing welding process on the microstructure and properties of the repaired surface.
  3. The development of a repair procedure that can be used in a production environment.

Conclusion

The research on the machining and surfacing welding process of a precision forging machine hammer head provides a practical solution to a common problem. The authors have developed a forging process that can produce a hammer head equivalent to an imported one, and a surfacing welding process that can repair worn hammer heads. The field trial results demonstrate that the proposed process is effective, with the hammer head producing 2000 axles before requiring repair. For the practicing engineer, this paper is a useful reference for anyone involved in the forging and repair of hammer heads. I would recommend that the study be extended to include a more extensive field trial and a detailed analysis of the microstructure and properties. The cost of a failed hammer head is not just the cost of the replacement; it is the cost of downtime, lost production, and the risk of catastrophic failure. A well-designed forging and repair process can extend the life of a hammer head by several cycles, providing significant savings.