EDC68 High-Hardness Wear-Resistant Surfacing Electrode: Formulation Optimization and Practical Welding Considerations
1. Literature Overview and the Hardness-Crack Tradeoff
This paper from the Journal of Welding (2001, Vol. 22, No. 5) describes the development of an EDC68 surfacing electrode with a hardness of 68-71 HRC. The authors used a design of experiments approach, specifically orthogonal regression, to optimize the electrode coating formulation. They established a regression equation for the hardness of the deposited metal, then optimized the formulation to achieve maximum hardness. They also analyzed the crack count in the weld beads to understand the effect of coating components on crack resistance.
This paper addresses one of the oldest problems in hardfacing: how to achieve high hardness without cracking. The relationship is fundamental. As hardness increases, the ductility and toughness of the deposited metal decrease, making it more susceptible to cracking. The challenge is to find the right balance of alloying elements in the coating to achieve maximum hardness while maintaining acceptable crack resistance.
2. Design of Experiments and Formulation Optimization
The authors used the ZWZY5 formulation design system to plan their experiments. They performed an orthogonal regression analysis to establish the relationship between coating components and deposited metal hardness. The key findings are:
| Coating Component | Effect on Hardness | Effect on Crack Count | Practical Consideration |
|---|---|---|---|
| Carbon | Increases | Increases | Primary hardening element |
| Chromium | Increases | Increases | Forms carbides |
| Molybdenum | Increases | Moderate | Solid solution strengthening |
| Nickel | Decreases | Decreases | Austenite former, improves toughness |
| Manganese | Moderate | Decreases | Deoxidizer, improves toughness |
The optimization process involved finding the formulation that maximized hardness while keeping the crack count within acceptable limits. The final EDC68 formulation achieved a hardness of 68-71 HRC with no cracking or only minor cracking when welded without preheat or with low-temperature preheat (150-350°C).
3. Practical Welding Considerations
The ability to weld without preheat or with only low-temperature preheat is a significant advantage. In many hardfacing applications, the component is large and preheating is difficult or impractical. The EDC68 electrode can be used in situations where other high-hardness electrodes would require preheating to 400°C or more.
However, the 68-71 HRC hardness comes with a caveat. This is an extremely hard material, and it is inherently brittle. In service, the layer may be subject to impact loading, thermal shock, or cyclic loading. The high hardness provides excellent wear resistance, but the low toughness means that the layer may crack or spall under impact.
The paper reports that the electrode can be used with preheat of 150-350°C. This is a wide range, and the optimal preheat depends on the size and geometry of the component. For small components, no preheat may be sufficient. For large components, the preheat should be at the higher end of the range to prevent cracking.
4. Production Application Considerations
For a production environment, the EDC68 electrode is suitable for applications where high hardness and wear resistance are required, such as:
- Crusher rolls and hammers
- Excavator teeth and buckets
- Mill liners and grinding media
- Pipe fittings and valves subject to abrasive wear
The electrode is a coated stick electrode, which means it is used with manual or semi-automatic welding. This limits the deposition rate compared to automatic processes, but it provides flexibility for welding in difficult positions and on complex geometries.
The coating of the electrode is critical to its performance. The coating contains the alloying elements that determine the hardness and crack resistance of the deposited metal. The coating also contains fluxing agents that protect the weld pool from oxidation and control the slag characteristics.
5. Critical Assessment and Study Insights
This paper is a good example of the application of design of experiments to electrode formulation. The authors have demonstrated a systematic approach to optimizing the coating composition, and the resulting electrode achieves excellent properties.
However, I would note the following limitations:
- The paper does not report the wear resistance of the deposited metal. Hardness is a proxy, but actual wear performance depends on the type of abrasive and the conditions of service.
- The paper does not report the impact toughness of the deposited metal. The high hardness suggests low toughness, but the actual value is not given.
- The paper does not discuss the effect of welding parameters on the properties. The hardness and crack count are likely to be sensitive to welding current, voltage, and travel speed.
6. Reference Value and Outlook
This paper is a useful reference for anyone involved in hardfacing with high-hardness electrodes. The formulation optimization approach is well-established, and the resulting electrode has a good combination of hardness and crack resistance.
For the practicing engineer, the key takeaway is that high hardness and crack resistance are not mutually exclusive. With careful formulation, it is possible to achieve hardness above 68 HRC with acceptable crack resistance. The key is to balance the carbon and alloy content to achieve the desired hardness while maintaining sufficient toughness to resist cracking.
My advice: if you are using this type of electrode in production, pay close attention to the preheat and interpass temperature. The 150-350°C range is wide, but the optimal value depends on the component size and geometry. Start with a preheat of 200°C and adjust based on the results. And always, always inspect the deposited layer for cracks before putting the component into service. A crack in a hardfacing layer is a potential failure point, and it will only get worse with time.
Zhuojin Pipe Fitting Co., Ltd