ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Fe-Cr-C-Mo Surfacing Alloy Layer: Characteristic Analysis

Literature Overview and Core Findings

This study by Jiang Jincheng, Liu Junyou, and colleagues from the University of Science and Technology Beijing examines the characteristics of Fe-Cr-C-Mo surfacing alloy layers, including the microstructure, hardness, and element distribution across the cross-section. The authors use optical microscopy, scanning electron microscopy, and energy-dispersive X-ray analysis to characterize the deposit.

The key finding is that the Fe-Cr-C-Mo surfacing layer has a high-hardness, good-toughness austenitic matrix and a wear-resistant martensitic phase. The martensite protects and supports the carbides, while the dispersed (Cr2.5Fe4.3Mo0.1)C3 and (Nb,Ti)C carbides provide high hardness and wear resistance, protecting the matrix. The surfacing layer has good crack resistance, good bonding with the substrate, and is not prone to spalling, which improves the overall wear resistance of the component.

Technical Interpretation from the Shop Floor

The Composite Structure of the Surfacing Layer

The Fe-Cr-C-Mo surfacing layer is a composite material, consisting of a matrix and a reinforcement phase. The matrix is austenite, which is tough and ductile, and it provides the support for the carbides. The reinforcement phase consists of M7C3-type carbides, specifically (Cr2.5Fe4.3Mo0.1)C3, and MC-type carbides, specifically (Nb,Ti)C.

The austenitic matrix is important because it provides toughness and ductility, which allows the surfacing layer to withstand impact and thermal cycling without cracking. The martensitic phase, which is present in some regions, provides additional hardness and wear resistance. The combination of austenite and martensite is unusual, but it provides a good balance of properties.

The carbides are the key to wear resistance. The M7C3 carbides are hard and wear-resistant, and the MC carbides are even harder. The dispersion of these carbides in the austenitic matrix provides a composite structure that resists abrasive wear while maintaining good toughness.

The Role of Molybdenum

Molybdenum is a key alloying element in this system. It is a strong carbide former, and it also provides solid solution strengthening of the matrix. The molybdenum content affects the type and amount of carbides that form, as well as the hardenability of the matrix.

In this alloy system, the molybdenum is incorporated into the M7C3 carbide, forming (Cr2.5Fe4.3Mo0.1)C3. This is interesting because it shows that molybdenum can substitute for chromium and iron in the M7C3 carbide, modifying its properties. The molybdenum also promotes the formation of the martensitic phase, which contributes to the hardness and wear resistance.

The Importance of the Bonding with the Substrate

The study emphasizes that the surfacing layer has good bonding with the substrate and is not prone to spalling. This is critical in service, because a surfacing layer that spalls off is worse than no surfacing at all. The spalling exposes the substrate to wear, and the hard, brittle pieces of the surfacing layer can cause damage to other components.

The good bonding is a result of the careful control of the welding parameters and the composition of the surfacing alloy. The dilution of the substrate into the surfacing layer must be controlled to avoid the formation of brittle phases at the interface. The preheating and interpass temperature must also be controlled to avoid cracking.

Engineering Practice and Lessons Learned

Case Study: Hot Rolling Mill Rolls

We once supplied Fe-Cr-C-Mo surfacing wire for hot rolling mill rolls. The rolls are subjected to severe wear and thermal cycling, and the surfacing layer must withstand both. The original specification called for a different alloy system, but we proposed the Fe-Cr-C-Mo system as an alternative.

The results were excellent. The Fe-Cr-C-Mo surfacing layer lasted about 20 percent longer than the original alloy, and the failure mode was different. The original alloy tended to crack and spall, while the Fe-Cr-C-Mo alloy wore more uniformly, with less cracking and spalling.