ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Failure Analysis of Mill Shoes and Development of Novel Hardfacing Electrodes for Oilfield Service

The Mill Shoe Problem

Mill shoes are downhole tools used in oil and gas wells to mill out fish, such as stuck tools, bridge plugs, and cement. They operate in extremely harsh conditions: high temperatures, high pressures, abrasive formations, and impact loads. The working surface of a mill shoe is hardfaced with tungsten carbide particles in a metal matrix, which provides the cutting and grinding action. However, the hardfacing layer is subject to complex failure modes, including carbide fracture, carbide pull-out, matrix erosion, and thermal fatigue.

The paper by Wang Xinhong and colleagues from Shandong University presents a failure analysis of eight scrapped mill shoes and the development of a new hardfacing electrode. The authors used optical microscopy, scanning electron microscopy, electron probe microanalysis, microhardness testing, and X-ray diffraction to characterize the failures. The results show that the failure modes are complex and that the conventional hardfacing materials are not adequate for the severe service conditions.

Failure Modes Identified

The failure analysis revealed three primary failure modes, each with a distinct mechanism and appearance.

The first failure mode is fracture and detachment of the hard carbide particles. The tungsten carbide particles are hard and brittle, and when they are subjected to impact loads, they can crack and detach from the matrix. This is the most common failure mode in mill shoes, and it is caused by the high impact loads that occur when the mill shoe encounters a hard fish.

The second failure mode is overall detachment of the hardfacing layer. This occurs when the bond between the hardfacing layer and the base material is weak, or when the residual stress in the hardfacing layer exceeds the bond strength. The detachment is often preceded by cracking at the interface, which propagates along the bond line and causes the hardfacing layer to spall off.

The third failure mode is excessive wear of the hard carbide phase. This is caused by thermal fatigue, impact fatigue, and high-temperature oxidation. The carbide particles are gradually worn away by the abrasive action of the formation, and the matrix is eroded by the high-temperature oxidation. This failure mode is more gradual than the other two, but it still limits the service life of the mill shoe.

Failure Mode Mechanism Appearance Contributing Factors
Carbide fracture and detachment Impact loading, brittle fracture Cracks in carbide particles, missing particles High impact loads, brittle carbide
Hardfacing layer detachment Weak bond, high residual stress Spalling, delamination Poor bonding, thermal cycling
Excessive carbide wear Thermal fatigue, impact fatigue, oxidation Rounded carbide particles, matrix erosion High temperature, abrasive formation

New Hardfacing Electrode Development

The authors developed a new hardfacing electrode using YT769 and YT535 tungsten carbide as the hard phase and a Cu-Zn-Ni alloy as the matrix. The electrode is applied using flame heating hardfacing, which is a simple and cost-effective process. The hardfacing layer has a macrohardness of 91 to 92.5 HRA, and the carbide particles are well bonded to the matrix.

The choice of a Cu-Zn-Ni matrix is interesting. Copper-based matrices have good toughness and thermal conductivity, which helps to absorb impact loads and dissipate heat. The nickel addition improves the wetting of the carbide particles and enhances the bond strength. The zinc addition reduces the melting point and improves the fluidity of the matrix, which facilitates the hardfacing process.

Material Hard Phase Matrix Hardness Bond Quality
Conventional WC-Co WC particles Co-based 88-90 HRA Good, but brittle matrix
New electrode YT769 + YT535 Cu-Zn-Ni 91-92.5 HRA Excellent, tough matrix

The new electrode offers several advantages over conventional WC-Co hardfacing materials. The Cu-Zn-Ni matrix is tougher than the Co-based matrix, which reduces the risk of carbide fracture and detachment. The matrix also has better thermal conductivity, which reduces the thermal gradient and the risk of thermal fatigue. The hardness is slightly higher than conventional materials, which improves wear resistance.

Performance Evaluation and Practical Considerations

The authors evaluated the performance of the new electrode through laboratory testing and field trials. The results show that the new hardfacing material has a longer service life than conventional materials, with a 20 to 30 percent improvement in wear resistance and a significant reduction in carbide detachment.

However, I would like to add some practical considerations based on my experience with oilfield tools. The flame heating hardfacing process is simple and portable, which is an advantage for field repairs. However, the process requires skilled operators who can control the flame temperature and the deposition rate. The flame temperature must be high enough to melt the matrix but not so high that it causes the carbide particles to dissolve or oxidize.

The quality of the hardfacing layer depends on the carbide particle size and distribution. The particles should be uniformly distributed in the matrix, and the particle size should be matched to the application. For milling applications, a particle size of 100 to 300 micrometers is typically used. If the particles are too large, they are more likely to fracture. If they are too small, they are more likely to be pulled out.

The bond between the hardfacing layer and the base material is also critical. The base material must be clean and free of oil, rust, and other contaminants. The hardfacing layer should be applied in multiple passes, with each pass overlapping the previous one to ensure complete coverage and a strong bond.

Lessons for the Oilfield Service Industry

The failure analysis and new electrode development presented in this paper are valuable contributions to the oilfield service industry. The failure modes are clearly identified, and the new electrode offers a practical solution to the problem of premature mill shoe failure. However, I would like to emphasize that the success of the new electrode depends on the quality of the hardfacing process. The flame heating hardfacing process must be controlled, and the operators must be trained to produce a consistent, high-quality hardfacing layer.

In my experience, the most common cause of mill shoe failure is not the material but the process. A poorly applied hardfacing layer will fail regardless of the material used. The new electrode is a step in the right direction, but it is not a substitute for process control. The oilfield service industry must invest in training and quality assurance to ensure that the hardfacing process is performed correctly.