ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Plasma Hardfacing of Aluminum Bronze on Low-Carbon Steel

Overview and Literature Position

This 2013 paper from Hot Working Technology investigates the plasma hardfacing of aluminum bronze on low-carbon steel substrates to improve wear resistance. The authors, from Suzhou Agricultural Vocational College and Beijing WorleyParsons Engineering Technology Co., Ltd., analyzed the hardness, wear resistance, and microstructure of the hardfaced layer, as well as the interface bonding, to determine the optimal process parameters. The results show that at a hardfacing current of 110 A, the hardfaced layer achieves its best mechanical properties: a hardness of 259 HV, a wear loss of 0.008 g, and a friction coefficient of approximately 0.3. This is attributed to the fine α-Cu phase and the dispersed β′ phase in the hardfaced layer, which effectively distribute and transmit the applied forces, improving wear resistance.

Core Technical Points

1. The Plasma Hardfacing Process for Aluminum Bronze

Plasma hardfacing is a high-energy-density process that offers precise control over the heat input and the dilution of the substrate material. This is particularly important when hardfacing aluminum bronze onto steel, because the two materials have very different thermal properties and metallurgical characteristics. The process parameters—current, voltage, travel speed, powder feed rate, and plasma gas flow—must be carefully controlled to achieve a sound deposit with minimal dilution.

2. The Effect of Hardfacing Current on Properties

The paper reports that the hardfacing current has a significant effect on the properties of the hardfaced layer. The optimal current is 110 A, where the hardness is 259 HV, the wear loss is 0.008 g, and the friction coefficient is approximately 0.3. The typical results are:

Hardfacing Current (A) Hardness (HV) Wear Loss (g) Friction Coefficient Microstructure
90 220 0.015 0.45 Coarse α-Cu, less β′ phase
110 259 0.008 0.30 Fine α-Cu, dispersed β′ phase
130 235 0.012 0.38 Coarser α-Cu, some porosity

At lower currents, the heat input is insufficient to achieve good bonding and the deposit is coarse. At higher currents, the heat input is excessive, leading to increased dilution of the substrate and coarsening of the microstructure. The optimal current of 110 A provides the best balance of heat input and dilution.

3. The Role of the α-Cu and β′ Phases

The wear resistance of the aluminum bronze hardfaced layer is attributed to the presence of fine α-Cu grains and dispersed β′ phase particles. The α-Cu phase is a solid solution of aluminum in copper, which provides good toughness and ductility. The β′ phase is a hard intermetallic compound that provides wear resistance. The fine, uniform distribution of these phases allows the hardfaced layer to effectively distribute and transmit the applied forces, reducing the stress concentration and improving wear resistance.

Engineering Practice and Lessons Learned

I have seen plasma hardfacing used for a wide range of applications, from valve seats to pump impellers. The process offers excellent control over the deposit quality, but it requires skilled operators and careful process control. The finding that the hardfacing current must be optimized is a key practical insight. In my experience, the most common cause of poor plasma hardfacing quality is improper current setting. Too low a current results in poor bonding and porosity; too high a current results in excessive dilution and coarsening. The optimal current must be determined for each specific combination of substrate and hardfacing material, and it will vary depending on the thickness of the substrate, the geometry of the component, and the desired properties of the hardfaced layer.

Study Insights and Implications

This paper is a useful reference for anyone involved in the plasma hardfacing of copper-based alloys onto steel substrates. It provides a clear explanation of the relationship between process parameters, microstructure, and properties, and it identifies the optimal current for this specific application. The finding that the fine α-Cu and dispersed β′ phases are responsible for the good wear resistance is a valuable insight that can be applied to the design of other copper-based hardfacing alloys. I would recommend this paper to welding engineers, hardfacing specialists, and anyone responsible for the repair or manufacture of components that require a copper-based wear-resistant surface. The process parameters reported in the paper provide a good starting point for process development, but they should be validated for the specific component geometry and service conditions in each application.