Submerged Arc Surfacing Repair of a 2-Ton Steam Hammer Anvil
The Service Failure and Repair Challenge
The paper by Zhou Hongbo, Li Zhisheng, and Yang Peizhen describes the repair of a 2-ton steam hammer anvil, which is a massive component that experiences severe thermal fatigue and impact loading. The anvil is made of cast steel, and the dovetail section is subjected to repeated impact from the hammer, which causes creep and thermal fatigue. The result is cracking and metal loss, and the anvil must be repaired or replaced.
The traditional repair method was manual arc welding, which required 3-4 welders working in shifts because of the large volume of weld metal needed. The repair area could be as large as 600 × 250 × 130 mm, which is a substantial amount of material. The manual arc welding process was slow and labor-intensive, and the quality of the repair depended on the skill of the welder.
The authors introduced submerged arc welding as an alternative, and the results were remarkable. The submerged arc welding process increased the productivity by more than five times, and the quality of the repair was significantly better. The anvil was repaired more than ten times, and the repairs were successful.
Submerged Arc Surfacing Process
Submerged arc welding is a process where the arc is completely submerged in a flux, which provides excellent protection from the atmosphere and allows for high deposition rates. The process is well-suited for surfacing large areas because it can deposit a large volume of metal in a short time.
| Parameter | Manual Arc Welding | Submerged Arc Welding |
|---|---|---|
| Deposition Rate | 1-2 kg/h | 5-10 kg/h |
| Number of Welders | 3-4 | 1-2 |
| Repair Time | 3-4 days | 1 day |
| Weld Quality | Dependent on skill | Consistent |
| Labor Intensity | High | Low |
The submerged arc welding process uses a solid wire or a flux-cored wire, and the flux is fed from a hopper. The wire diameter is typically 3.2-5.0 mm, and the welding current is in the range of 300-600 A. The arc voltage is 25-35 V, and the travel speed is 20-40 cm/min.
| Parameter | Value |
|---|---|
| Wire Diameter | 4.0 mm |
| Welding Current | 350-450 A |
| Arc Voltage | 28-32 V |
| Travel Speed | 25-35 cm/min |
| Preheat Temperature | 200-250 °C |
| Interpass Temperature | 250-300 °C |
The preheat temperature is critical for a large component like an anvil. The anvil has a mass of several tons, and the heat input from the welding process is not sufficient to maintain the temperature. A preheat of 200-250 °C is recommended, and the temperature must be monitored throughout the welding process. If the temperature drops below the preheat level, the weld metal will cool too quickly and form a brittle structure.
Quality Control and Inspection
The quality of the repair depends on the control of the welding process and the inspection of the completed repair. The authors emphasise that the weld metal must be free from cracks, porosity, and lack of fusion. The inspection methods are visual inspection, ultrasonic testing, and magnetic particle testing.
| Inspection Method | Purpose | Acceptance Criteria |
|---|---|---|
| Visual Inspection | Surface defects | No cracks, no porosity |
| Ultrasonic Testing | Subsurface defects | No indications above 2 mm equivalent |
| Magnetic Particle Testing | Surface cracks | No linear indications |
The ultrasonic testing is particularly important for a large component like an anvil because it can detect subsurface defects that are not visible on the surface. The inspection should be performed after the repair is complete and the anvil has cooled to ambient temperature.
Practical Lessons and Engineering Insights
The paper by Zhou Hongbo and his colleagues is a valuable contribution to the field of repair welding. It demonstrates that submerged arc welding can be used effectively for the repair of large components, and it provides a clear comparison between the traditional manual arc welding and the submerged arc welding process.
One of the practical lessons I have learned from similar repairs is that the preheat and interpass temperature control is the most critical factor. A large component like an anvil has a high thermal mass, and the temperature can drop quickly if the welding is interrupted. The welder must be disciplined about monitoring the temperature and applying additional preheat if necessary.
Another lesson is that the welding process must be planned carefully to avoid distortion. The anvil is a large component, and the welding heat can cause it to warp. The welding sequence should be designed to balance the heat input and minimise distortion. The authors do not discuss this in detail, but it is a practical consideration that cannot be ignored.
The submerged arc welding process is an excellent choice for the repair of large components because it offers high deposition rates and consistent quality. The paper provides a clear description of the process parameters and the quality control requirements, and it is a valuable reference for any engineer who is faced with a similar repair challenge.