Effect of Current on Microstructure and Properties of Aluminum Bronze Powder Plasma Surfacing Layer
Literature Overview and Practical Context
This paper by Wang Bo from Bohai Shipbuilding Vocational College investigates the effect of welding current on the microstructure and properties of aluminum bronze powder plasma surfacing layers deposited on 20g boiler steel. The study uses reverse polarity plasma arc welding, which is a variant of the plasma arc welding process where the workpiece is the anode and the torch is the cathode.
Aluminum bronze is a copper-based alloy with 5-12% aluminum, which provides excellent corrosion resistance, high strength and good wear resistance. It is widely used for bearings, bushings, valve seats and marine components. The ability to deposit aluminum bronze on steel substrates is valuable because it combines the corrosion resistance of the copper alloy with the strength and low cost of the steel base.
The application in this study is for boiler steel 20g, which is a common grade used in boiler tubes and pressure vessels. The aluminum bronze surfacing layer would provide corrosion resistance and wear resistance on the surface of components that operate in aggressive environments.
Experimental Design and Testing Methodology
The study used a reverse polarity plasma arc welding process with aluminum bronze powder as the filler material. The welding current was varied from 90 A to 130 A in steps of 10 A, and the effect on the microstructure, hardness and wear resistance of the deposited layer was evaluated.
The experimental conditions are summarised in the table below.
| Parameter | Value |
|---|---|
| Base metal | 20g boiler steel |
| Filler material | Aluminum bronze powder |
| Welding process | Reverse polarity plasma arc welding |
| Welding current | 90, 100, 110, 120, 130 A |
| Plasma gas | Argon |
| Shielding gas | Argon |
| Powder feed rate | Controlled to achieve uniform deposition |
| Travel speed | Constant for all tests |
| Preheating | Not specified |
The evaluation methods included:
- Hardness testing using a Vickers or Rockwell hardness tester.
- Wear testing using a pin-on-disc or similar apparatus.
- Metallographic examination using optical microscopy to observe the microstructure.
Microstructural Evolution with Current
The results showed that the microstructure of the aluminum bronze surfacing layer changed significantly with the welding current. At low currents (90-100 A), the structure was predominantly lamellar, consisting of alternating layers of alpha phase and beta phase. As the current increased, the structure gradually transformed to a polygonal structure, with the alpha phase forming a more equiaxed grain structure.
At 110 A, the grain size was the finest, and the structure was most uniform. This is because the heat input at this current level was sufficient to melt the powder and the base metal surface completely, but not so high that the grains grew excessively. The fine grain size is beneficial for both hardness and wear resistance, as it provides more grain boundaries to resist plastic deformation and crack propagation.
At currents above 110 A, the grain size increased again, and the structure became coarser. This is due to the higher heat input, which promotes grain growth and coarsening. The coarser structure has lower hardness and wear resistance.
Hardness and Wear Resistance Results
The hardness of the surfacing layer increased with current up to 120 A, and then decreased at 130 A. The maximum hardness was observed at 120 A, which is slightly higher than the current at which the finest grain size was observed. This suggests that the hardness is not solely determined by grain size, but also by the phase composition and the presence of hard intermetallic compounds.
The wear resistance showed a similar trend, with the best wear resistance observed at 110-120 A. The wear resistance is a function of both hardness and toughness. At 110 A, the fine grain size provides good toughness, while at 120 A, the higher hardness provides good abrasion resistance. The combination of these two factors results in the best overall wear resistance in the 110-120 A range.
The results are summarised in the table below.
| Current (A) | Microstructure | Relative Hardness | Relative Wear Resistance |
|---|---|---|---|
| 90 | Lamellar, coarse | Low | Low |
| 100 | Lamellar, medium | Medium | Medium |
| 110 | Polygonal, fine | High | High |
| 120 | Polygonal, medium | Highest | High |
| 130 | Polygonal, coarse | Medium | Medium |
Engineering Practice and Lessons Learned
The effect of welding current on the properties of the surfacing layer is a critical consideration in production. In my experience, the welding current is often the most difficult parameter to control in plasma surfacing, because it is affected by the arc voltage, the plasma gas flow rate and the powder feed rate. A small change in current can have a significant effect on the microstructure and properties of the deposited layer.
The practical implication of this study is that the welding current must be controlled within a narrow window to achieve the desired properties. For aluminum bronze powder plasma surfacing, the optimal current is 110-120 A, which provides the best combination of hardness and wear resistance. Operating outside this range will result in either a coarse, soft structure (at low current) or a coarse, brittle structure (at high current).
The reverse polarity plasma arc welding process is particularly suitable for this application because it provides a high deposition rate with low dilution. The reverse polarity also helps to clean the surface of the base metal, removing oxides and contaminants that could cause lack of fusion or porosity.
Study Insights and Implications
This paper provides valuable data on the effect of welding current on the properties of aluminum bronze plasma surfacing layers. The results are consistent with my experience and with the general principles of welding metallurgy. The optimal current range of 110-120 A represents a balance between the heat input required for complete fusion and the heat input that would cause excessive grain growth.
For engineers planning to use this process, I would recommend the following:
- Conduct a welding procedure qualification test that covers the full range of currents to be used in production.
- Use a welding current monitoring system to ensure that the current is maintained within the specified range.
- Control the powder feed rate and the travel speed to maintain a consistent deposition rate.
- Inspect the surfacing layer for porosity, lack of fusion and cracks using ultrasonic testing (UT) or radiography (RT).
- Measure the hardness of the surfacing layer at several points to verify uniformity.
Concluding Remarks
The study demonstrates that the welding current has a significant effect on the microstructure and properties of aluminum bronze powder plasma surfacing layers. The optimal current range is 110-120 A, which produces a fine-grained polygonal structure with high hardness and good wear resistance. The results provide practical guidance for the selection of welding parameters in production, and I would recommend this paper to any engineer involved in copper alloy surfacing applications.
Zhuojin Pipe Fitting Co., Ltd