ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Failure Analysis of Co-Based Superalloy and Optimization of TIG Cladding Process

Literature Overview and the Failure Problem

This paper by Guo Ying and colleagues from Beijing Aerospace Chemical Engineering and Environmental Protection Technology Co., Ltd. addresses a specific and serious industrial problem: the end-face cracking failure of the outer spray nozzle of a pure oxygen burner in a coal chemical plant. The component is made of a cobalt-based superalloy, UMCo50, and it fails by cracking at the end face during service.

The authors conduct a thorough failure analysis, examining the microstructure and phase composition of the failed surface material, and identifying the different failure modes. Based on this analysis, they develop a TIG cladding process using UMCo50 filler material on the same substrate, and they optimise the process using an orthogonal experimental design.

Failure Analysis Findings: The Root Cause

The failure analysis reveals that the outer spray nozzle fails by end-face cracking. The cracking is caused by a combination of thermal fatigue and oxidation. The nozzle operates at high temperature in an oxygen-rich environment, and the end face is subjected to repeated thermal cycling. This causes thermal fatigue cracks to initiate at the surface and propagate into the material.

The microstructure of the failed surface shows signs of oxidation and carbide coarsening. The cobalt-based superalloy relies on a fine dispersion of carbides for its high-temperature strength. During service, the carbides coarsen, which reduces the strength and increases the susceptibility to cracking. The oxidation depletes the surface of chromium, which reduces the oxidation resistance and accelerates the degradation.

The failure analysis also identifies different damage forms, suggesting that the cracking is not a single-mode failure but a combination of several mechanisms. This is typical of high-temperature components in aggressive environments. The root cause is the combination of thermal cycling, oxidation and carbide coarsening, which together lead to end-face cracking.

Orthogonal Experimental Design and Process Optimisation

The authors use an orthogonal experimental design to optimise the TIG cladding process. The factors considered are welding current, cladding speed, interpass temperature and number of cladding layers. The response variable is the quality of the cladding, which is assessed by visual inspection, crack detection and hardness measurement.

The optimal process parameters are identified as: welding current 120 A, cladding speed 10-11 cm/min, interpass temperature 60 ± 10 °C, and 2-3 cladding layers. These parameters produce a cladding layer that is crack-free, well-bonded and with acceptable hardness.

Parameter Optimal Value Effect on Quality
Welding current 120 A Moderate heat input, good fusion without excessive dilution
Cladding speed 10-11 cm/min Balanced deposition rate and heat input per unit length
Interpass temperature 60 ± 10 °C Low enough to prevent cracking, high enough to avoid cold cracking
Number of layers 2-3 Sufficient thickness for repair, without excessive thermal stress

Why These Parameters Work

The welding current of 120 A is moderate for TIG cladding. It provides enough heat to melt the filler wire and achieve good fusion with the substrate, but not so much heat that the dilution rate becomes excessive. High dilution would contaminate the cladding with substrate material and reduce its high-temperature properties.

The cladding speed of 10-11 cm/min is relatively slow, which gives a high heat input per unit length. This is beneficial for cladding because it ensures good fusion and a smooth bead profile. However, too slow a speed can cause excessive heat input and distortion.

The interpass temperature of 60 ± 10 °C is critical. If the interpass temperature is too high, the accumulated heat causes grain growth and carbide coarsening in the cladding, which reduces its strength. If the interpass temperature is too low, the cladding cools too quickly and thermal stress causes cracking. The 60 °C interpass temperature is a compromise that maintains the cladding temperature within a safe range.

The 2-3 layer thickness is also important. A single layer may be too thin to provide adequate repair, while more than 3 layers may cause excessive thermal stress and distortion. The 2-3 layer range provides sufficient thickness without over-heating the component.

Practical Implications for Repair Welding

This paper is a textbook example of how to approach a repair welding problem. The first step is to understand the failure mechanism. Without a proper failure analysis, you are guessing at the root cause, and guessing leads to ineffective repairs. The authors did the right thing by starting with a thorough failure analysis before developing the repair process.

The second step is to optimise the repair process using a systematic method. The orthogonal experimental design is an efficient way to identify the optimal process parameters with a limited number of experiments. The range analysis method allows you to determine the relative importance of each factor and to identify the optimal combination.

The third step is to verify the optimised process in actual production. The authors report that the optimal process was verified in actual production, which is the ultimate test. A process that works in the laboratory but fails in production is worthless.

In my experience, repair welding of high-temperature components is a high-risk activity. The component has already been in service, and its material properties may have degraded. The repair weld must be compatible with the degraded material, and the process must be carefully controlled to avoid introducing new defects. This paper demonstrates that a systematic approach can produce a reliable repair process.

Key Questions and Reflections

The paper focuses on TIG cladding, but it does not compare this process with other cladding techniques such as plasma cladding, laser cladding or friction surfacing. Each technique has its own advantages and disadvantages. TIG cladding is simple and inexpensive, but it has a relatively high heat input and dilution rate. Plasma cladding has a lower heat input and dilution rate, but it is more complex and expensive. Laser cladding has the lowest heat input and dilution rate, but it requires expensive equipment.

I would also question the long-term performance of the repair. The paper reports that the optimal process was verified in actual production, but it does not provide data on the service life of the repaired component. A repair that lasts for a few months is not a successful repair. I would want to see at least 12 months of service data before accepting the process.

The failure analysis identifies oxidation and carbide coarsening as contributing factors, but it does not provide quantitative data on the extent of oxidation or the degree of carbide coarsening. This makes it difficult to assess the severity of the degradation and to determine the remaining life of the component.

Study Insights and Reference Value

This paper is a valuable contribution to the field of repair welding of high-temperature components. It demonstrates the importance of failure analysis in understanding the root cause of failure, and it shows how a systematic process optimisation can produce a reliable repair process. The orthogonal experimental design is an efficient tool for process optimisation, and the range analysis method is a simple and effective way to identify the optimal parameters.

For the pipe and fitting industry, the key takeaway is that repair welding is a specialised activity that requires a systematic approach. You cannot simply weld over a crack and hope for the best. You need to understand why the component failed, select the appropriate repair process, optimise the process parameters and verify the repair in actual service.

The reference value of this work is highest for engineers working on repair and maintenance of high-temperature components in the chemical, petrochemical and power generation industries. For the pipe industry, it is a reminder that even the most carefully designed components can fail in service, and that a well-executed repair can extend the service life significantly.