Introduction

Medium-carbon steel 45 (equivalent to AISI 1045) is widely used for shafts, gears, and structural components that require surface wear resistance. Hardfacing is a common method to extend service life, but the choice of filler material and welding parameters directly determines the deposit's performance. The study by Xie et al. compares two electrodes: CHR172 (Cr-Ni-Mo type) and CHR132 (Cr-Mo type), both martensitic stainless steel grades. This note distils the findings and connects them to practical hardfacing decisions on the shop floor.

Experimental Procedure and Results

The researchers performed manual arc welding (SMAW) on 45 steel plates using each electrode. Welding current was 120–140 A, voltage 22–26 V, and travel speed 15–20 cm/min. After welding, samples were sectioned, polished, etched with a 4% nital solution, and examined under an optical microscope. Microhardness was measured using a Vickers tester with a 100 g load.

Electrode Deposit Structure Average Hardness (HV) Approx. HRC
CHR172 Martensite + retained austenite + carbides 450–500 45–50
CHR132 Martensite + fine carbides 380–420 40–45

The CHR172 deposit exhibited a finer martensitic matrix with more uniform carbide distribution, attributed to the higher nickel and molybdenum content. The heat-affected zone (HAZ) of the base metal showed a martensitic layer due to rapid cooling, with hardness peaking near the fusion line. The study also noted that increasing welding current increased dilution, which reduced the hardness of the deposit because of carbon pickup from the base metal.

Practical Implications

For applications requiring maximum abrasion resistance, CHR172 is the better choice. Its higher hardness and corrosion resistance make it suitable for mining equipment, crusher hammers, and pump impellers. CHR132, with lower hardness but better toughness, is preferable where impact loading is significant, such as in gear teeth or rail components. In my experience, selecting the wrong electrode for a given service condition is a common mistake. A client once specified CHR132 for a coal crusher hammer; the deposit wore out in three months. Switching to CHR172 extended life to over a year.

Welding parameters are equally critical. Preheat at 200–300°C is recommended for 45 steel to prevent HAZ cracking, especially when using martensitic electrodes. Post-weld tempering at 200–400°C can reduce residual stress and improve toughness. On the shop floor, I insist on documenting actual current, voltage, and travel speed for each pass, because deviations of more than 10% from the procedure can change hardness by 5–10 HRC.

Summary

The microstructure and hardness of hardfacing deposits on 45 steel are directly influenced by electrode composition and welding parameters. CHR172 provides higher hardness and wear resistance, while CHR132 offers better impact toughness. The practical lesson is to match the electrode to the service environment and to control the welding process rigorously. A well-executed hardfacing can triple the service life of a component, but a poorly executed one can introduce cracking and premature failure.