Strip Cladding Process for Lock Hopper Cone

Background and Material Analysis

The lock hopper is a critical component in coal gasification systems, where it operates under high pressure and corrosive conditions. The cone section of the lock hopper is particularly demanding, as it must withstand both the internal pressure and the abrasive and corrosive effects of coal ash and syngas. The base material is 16MnR, a low-alloy pressure vessel steel with a yield strength of 345 MPa, and the cladding material is 00Cr17Ni14Mo2, a low-carbon austenitic stainless steel with excellent corrosion resistance. The challenge is to apply a uniform, crack-free cladding layer on the conical surface, which has a steep taper and a complex geometry that makes conventional welding difficult. The authors of this study performed a thorough process analysis and developed a strip cladding process with a custom-designed tooling fixture to handle the conical geometry.

Process Selection and Tooling Design

The selection of the cladding method was based on several factors: the cladding thickness of 6 mm, the requirement for a smooth and uniform surface, and the need for high deposition efficiency. Strip cladding was chosen over wire cladding because it offers a higher deposition rate, lower dilution, and a more uniform bead profile. The strip electrode used was 60 mm wide, with a composition matching 00Cr17Ni14Mo2, and a matching agglomerated flux. The critical challenge was the conical geometry of the workpiece. The cone has an apex angle of approximately 60 degrees, and the cladding must be applied in a spiral pattern from the bottom to the top. A conventional strip cladding head cannot follow the conical surface without the torch angle changing, which would cause uneven bead width and penetration. The authors designed a custom tooling fixture that holds the cone in a rotating chuck and tilts the cladding head to maintain a constant angle relative to the cone surface. The fixture also includes a water-cooled copper backing plate on the outside of the cone to control heat input and prevent distortion.

Parameter Value / Range Remarks
Base material 16MnR 345 MPa yield strength
Cladding material 00Cr17Ni14Mo2 Low-carbon austenitic stainless
Cladding method Strip cladding (ESW) 60 mm wide strip
Cladding thickness 6 mm Two layers of 3 mm
Strip electrode 60 mm wide Matched composition
Welding current 600–800 A DC reverse polarity
Arc voltage 24–28 V Stable arc
Travel speed 12–16 cm/min Spiral pattern
Preheat 100°C Prevents HAZ cold cracking
Interpass temperature ≤150°C Controls distortion

Welding Procedure Qualification

The welding procedure qualification (WPQ) was performed according to ASME Section IX, with test coupons cut from a representative cone section. The qualification included visual inspection, liquid penetrant testing (PT), ultrasonic testing (UT), and metallographic examination. The cladding was applied in two layers, with the first layer at a current of 650 A and the second layer at 700 A to achieve the required thickness and dilution. The deposit hardness was measured at 180 to 200 HV, which is typical for austenitic stainless steel, and the ferrite content was controlled at 3% to 8% by volume to prevent hot cracking. The metallographic examination showed a sound bond between the cladding and the base metal, with no cracks, porosity, or slag inclusions. The cladding interface was free of carbide precipitation, which is critical for corrosion resistance in the service environment. The WPQ was accepted, and the process was approved for production.

Production Application and Quality Control

The production application involved cladding the cone sections of two lock hoppers for a coal gasification plant. The tooling fixture was set up, and the cladding was applied in a spiral pattern, with each pass overlapping the previous one by 30% to 40% to ensure complete coverage. The cladding thickness was verified at 6 mm ± 0.5 mm using an ultrasonic thickness gauge. After cladding, the cone was subjected to a post-weld heat treatment (PWHT) at 620°C for 2 hours to relieve residual stresses, followed by a 100% PT and UT inspection. The results were satisfactory, with no indications of cracking or lack of fusion. The cone was then machined to final dimensions and hydrostatically tested at 1.5 times the design pressure. The test was successful, and the lock hopper was shipped to the site. The authors noted that the total cladding time was reduced by 30% compared to the previous method, which used manual wire welding, and the surface quality was significantly improved, reducing the machining allowance and grinding time.

Conclusion

This study demonstrates that strip cladding, with a properly designed tooling fixture, is a viable and efficient method for cladding conical components such as lock hopper cones. The key to success is the tooling design, which maintains a constant torch angle and ensures uniform bead geometry on the conical surface. The WPQ confirmed the metallurgical quality of the cladding, and the production application proved the process is reliable and cost-effective. For our industry, this is a valuable lesson in process engineering: the geometry of the workpiece should not be an afterthought but a primary consideration in process selection. I would recommend this approach to any fabricator dealing with complex geometries, as the tooling investment pays for itself in reduced cycle time and improved quality.