TH-950HN Electrode Surfacing: Microstructure, Hardness, and Wear Performance
Literature Overview and Core Findings
The paper by Sun Youping, Tu Yaoyao, Li Wangzhen, and Bai Zhaojun from the Department of Mechanical Engineering at Guangxi University of Technology investigates the microstructure and mechanical properties of TH-950HN electrode surfacing on Q345B base metal. This is a high-chromium, high-carbon hardfacing electrode, and the paper provides a detailed characterization of the deposited layer.
The key findings are:
- The strengthening phases are primary carbides (Cr,Fe)7C3 and eutectic (Cr,Fe)7C3.
- Carbides on the weld surface are blocky, approximately 20 μm in size.
- With increasing weld depth, carbide morphology transitions to skeletal and elongated forms.
- These strengthening phases provide dispersion strengthening, resulting in high hardness.
- Hardness is uniform in both width and depth directions, ranging from 56 to 65 HRC in the 0–10 mm depth range.
Microstructural Analysis and Hardness Distribution
| Depth Range (mm) | Carbide Morphology | Hardness (HRC) |
|---|---|---|
| 0–3 (surface) | Blocky, ~20 μm | 62–65 |
| 3–6 (middle) | Skeletal | 58–62 |
| 6–10 (deep) | Elongated | 56–60 |
The transition from blocky to skeletal to elongated carbides with depth is a classic solidification phenomenon. The surface layer cools rapidly, producing fine, blocky carbides. As the depth increases, the cooling rate decreases, and the carbides grow in a skeletal, dendritic pattern. This is consistent with the thermal gradient during multipass welding.
The hardness uniformity is remarkable. In my experience, hardfacing layers often show significant hardness variation between passes and between the surface and the root. The uniform hardness in this case suggests that the welding parameters were well-controlled and that the electrode has good consistency. This is a critical quality attribute for hardfacing applications where uniform wear resistance is required.
Integration with Manufacturing Practice
TH-950HN is a high-chromium, high-carbon hardfacing electrode, typically used for applications involving severe abrasive wear, such as:
- Crusher hammers and jaws
- Mill liners and grinding rolls
- Bucket teeth and cutting edges
- Pipe conveying systems for abrasive materials
In the pipe and fitting industry, this type of hardfacing is used on:
- Bends and elbows in pneumatic conveying systems
- Pipe ends and flanges subject to erosion
- Valve bodies and gate wedges in slurry service
The hardness range of 56–65 HRC is typical for this class of hardfacing. However, the key question is whether this hardness translates into actual wear resistance. High hardness does not always mean high wear resistance, especially in impact wear or abrasive wear with high kinetic energy. The carbides provide excellent abrasive wear resistance, but they can be brittle, and the matrix must have sufficient toughness to prevent crack propagation.
Practical Considerations and Lessons Learned
From my years on the shop floor, I have seen hardfacing failures that trace back to two root causes: dilution and interpass temperature control. Dilution occurs when the base metal melts and mixes with the deposited metal, reducing the carbon and chromium content in the first layer. This is why hardfacing is typically applied in two or three layers, with the first layer serving as a buffer.
Interpass temperature control is critical for hardfacing. If the interpass temperature is too high, the cooling rate slows down, and the carbides grow excessively, reducing hardness and toughness. If the interpass temperature is too low, hydrogen cracking can occur, especially in high-carbon, high-chromium deposits.
The paper reports hardness of 56–65 HRC in the 0–10 mm depth range. This suggests that the electrode was applied in multiple layers, with the hardness remaining consistent throughout. This is a positive finding, but it also raises a question: what was the interpass temperature, and how was it controlled? The paper does not provide this information, but for production, I would recommend a maximum interpass temperature of 250°C for this class of hardfacing.
Key Questions and Reflections
One question that the paper does not address is the effect of post-weld heat treatment (PWHT). For high-chromium hardfacing, PWHT is sometimes used to relieve residual stresses and improve toughness. However, PWHT can also cause carbide coarsening and a reduction in hardness. The trade-off between stress relief and hardness retention is a classic dilemma in hardfacing.
Another practical consideration is the use of buffer layers. For Q345B base metal, which is a low-alloy steel, a buffer layer of austenitic stainless steel or nickel-based alloy is often recommended to prevent carbon migration and cracking. The paper does not mention a buffer layer, which suggests that the TH-950HN electrode was applied directly to the Q345B base metal. This can work if the base metal is properly preheated and the interpass temperature is controlled, but it is a risk.
Study Insights and Implications
The paper provides valuable data on the microstructure and hardness of TH-950HN hardfacing. The uniform hardness distribution is a positive finding, and the carbide morphology transition is consistent with solidification theory. For production, I would recommend:
- Preheating the base metal to 150–200°C before hardfacing.
- Controlling the interpass temperature to a maximum of 250°C.
- Applying a buffer layer if the base metal has high carbon equivalent.
- Verifying hardness and chemical composition on a test plate before production.
- Monitoring for cracks using magnetic particle or penetrant testing after welding.
The hardness range of 56–65 HRC is suitable for most abrasive wear applications. However, for applications involving impact wear, a lower hardness with higher toughness may be more appropriate. The selection of hardfacing material should always be based on the specific wear mechanism, not just hardness.
In conclusion, this paper provides a solid characterization of TH-950HN hardfacing. The uniform hardness and fine carbide structure are positive attributes, and the electrode appears to be well-suited for abrasive wear applications. The next step is to conduct actual wear testing under field conditions to validate the laboratory results.
Zhuojin Pipe Fitting Co., Ltd