ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Continuous Casting Roller Surfacing Technology: A Status Review and Practical Assessment

Literature Overview and Technical Context

This paper by Yang Zhengyong from Baosteel Equipment Maintenance Company provides a status review of surfacing technology for continuous casting rollers. The continuous casting process is a critical step in steel production, and the rollers play a key role in supporting and guiding the cast strand. The rollers operate under severe conditions: they are subjected to high temperatures, thermal cycling, mechanical loading, and abrasive wear. The service life of the rollers directly affects the productivity and cost of the continuous casting process, and surfacing is the primary method for extending their life.

The paper reviews the current state of the art in roller surfacing, covering the types of surfacing materials, the welding processes used, and the challenges associated with the repair and refurbishment of these components. The context is the rapid growth of China's steel production, which has increased the demand for continuous casting and, consequently, for roller surfacing services.

Technical Interpretation: The Service Conditions and Failure Modes

Continuous casting rollers fail by a combination of mechanisms, and the dominant failure mode depends on the location of the roller in the machine. The rollers in the mold region are subjected to the highest temperatures and the most severe thermal cycling, and they fail primarily by thermal fatigue cracking. The rollers in the secondary cooling zone are subjected to a combination of thermal fatigue and mechanical loading, and they fail by a combination of cracking and wear. The rollers in the straightening and withdrawal section are subjected to high mechanical loads and abrasive wear, and they fail primarily by wear and deformation.

The surfacing materials used for these rollers must be selected based on the dominant failure mode. For thermal fatigue resistance, a material with a low thermal expansion coefficient and high thermal conductivity is preferred. For wear resistance, a material with high hardness and good abrasive wear resistance is required. In practice, a compromise is often necessary, and the surfacing material is selected to provide the best combination of properties for the specific application.

Surfacing Materials and Process Selection

Material Type Typical Hardness Key Properties Application
Martensitic stainless steel (13Cr type) 40-50 HRC Good thermal fatigue resistance, moderate wear resistance Secondary cooling zone rollers
Tool steel (5Cr-2Mo type) 50-55 HRC High wear resistance, moderate thermal fatigue resistance Straightening rollers
Nickel-based alloy 35-45 HRC Excellent thermal fatigue resistance, good corrosion resistance Mold region rollers
Composite (hardfacing over buffer layer) 50-60 HRC Best combination of toughness and wear resistance High wear applications

The table above summarizes the typical surfacing materials used for continuous casting rollers. The selection of the material is a critical decision that affects both the service life and the cost of the roller. In my experience, the martensitic stainless steel type is the most common choice for secondary cooling zone rollers, because it provides a good balance of thermal fatigue resistance and wear resistance at a reasonable cost.

The welding process used for roller surfacing is typically submerged arc welding (SAW) with a single wire or a twin wire configuration. The SAW process is preferred because it provides high deposition rates and a smooth, uniform surface finish. Other processes such as flux-cored arc welding (FCAW) and plasma transferred arc welding (PTAW) are also used, but they are less common for this application.

Process Control and Quality Assurance

The quality of the surfacing layer is critical to the service life of the roller. The key process parameters are:

  1. Preheat temperature: The rollers are typically preheated to 200-300 C before surfacing to prevent cracking. The preheat temperature must be maintained throughout the welding process, and the interpass temperature must be controlled to avoid overheating.
  2. Welding current and voltage: These parameters determine the deposition rate and the penetration depth. A higher current increases the deposition rate but also increases the heat input, which can cause distortion and cracking.
  3. Travel speed: The travel speed affects the bead width and the heat input. A slower travel speed increases the heat input and can cause excessive dilution, while a faster travel speed can cause lack of fusion.
  4. Wire diameter and composition: The wire diameter affects the deposition rate and the bead shape. The wire composition must be matched to the desired surfacing material.

The quality of the surfacing layer is verified by non-destructive testing, including ultrasonic testing for the detection of lack of fusion and cracks, and magnetic particle testing for the detection of surface cracks. The hardness of the surfacing layer is also measured to verify that it meets the specification.

Common Defects and Countermeasures

Defect Root Cause Countermeasure
Cracking High residual stress, improper preheat Increase preheat temperature, use a buffer layer, control interpass temperature
Porosity Moisture in the flux, contamination on the surface Dry the flux, clean the surface before welding
Lack of fusion Low welding current, high travel speed Increase welding current, reduce travel speed
Distortion Excessive heat input, improper welding sequence Use a balanced welding sequence, reduce heat input
Undercut High welding current, high travel speed Reduce welding current, reduce travel speed

The table above lists the common defects in roller surfacing and the corresponding countermeasures. Cracking is the most serious defect because it can lead to catastrophic failure of the roller. The use of a buffer layer is a common practice for high hardness surfacing materials, because it provides a transition zone between the base metal and the hardfacing layer, reducing the residual stress and preventing cracking.

Engineering Practice Cases and Lessons Learned

In my experience, the most common problem in roller surfacing is distortion. The rollers are long and slender, and the heat input from the welding process causes them to bend. The distortion can be controlled by using a balanced welding sequence, where the welding is alternated between the two sides of the roller. However, this requires a high degree of process control and operator skill.

I recall a case where a batch of rollers was rejected because the distortion exceeded the allowable limit. The root cause was that the welding sequence was not properly balanced, and the rollers were welded on one side before the other. The fix was to implement a strict welding sequence that alternated between the two sides, and to use a lower heat input to reduce the thermal gradient.

Another common problem is the lack of fusion between the surfacing layer and the base metal. This is often caused by contamination on the surface of the roller, such as oil, grease, or scale. The surface must be thoroughly cleaned before welding, and the cleaning must be verified by visual inspection or magnetic particle testing.

Study Insights and Practical Implications

This paper provides a useful overview of the current state of the art in continuous casting roller surfacing, but it is a status review rather than a detailed technical investigation. The value of the paper lies in its comprehensive coverage of the materials, processes, and challenges associated with roller surfacing.

The key insight for the practicing engineer is that the selection of the surfacing material and the welding process must be based on the specific service conditions of the roller. There is no universal solution, and each application requires a careful analysis of the failure mode and the operating conditions.

The economic aspect is also important. The cost of surfacing a roller must be compared to the cost of a new roller, and the decision to repair or replace must be based on the expected service life and the total cost of ownership. In many cases, surfacing is the more economical option, but this depends on the condition of the roller and the availability of the surfacing equipment and materials.

Reference Value and Outlook

This paper is a valuable reference for engineers involved in the maintenance and repair of continuous casting rollers. It provides a good overview of the current practice and highlights the key challenges and opportunities.

Looking forward, the development of new surfacing materials with improved thermal fatigue resistance and wear resistance is an active area of research. The use of composite materials, where hard particles are embedded in a tough matrix, is a promising approach, but the manufacturing process is more complex and the cost is higher.

In conclusion, continuous casting roller surfacing is a mature technology that plays a critical role in the steel industry. The key to success is the proper selection of the surfacing material and the welding process, combined with rigorous process control and quality assurance. The paper provides a good foundation for understanding the current state of the art, and it highlights the importance of practical experience in achieving optimal results. The lessons learned from shop floor practice are invaluable, and they should be incorporated into the design and qualification of any roller surfacing procedure.