Hardfacing of Small-Diameter 4Cr10Si2Mo Exhaust Valves with Cobalt-Based Alloy No. 1

Literature Overview and Context

The paper by Yang Zheng and Dai Mingfa, published in Diesel Engine in 1992, addresses a persistent manufacturing problem encountered at the Anqing Marine Diesel Engine Factory. The subject is the manual TIG hardfacing of small-diameter exhaust valve discs made from 4Cr10Si2Mo martensitic heat-resistant steel, using cobalt-based alloy No. 1 as the filler material. The specific engine is the Daihatsu DS-18, a marine diesel engine where the exhaust valve disc diameter is relatively small, the required hardfacing layer is thin, and the weld quality demands are stringent.

From my years on the shop floor, I can tell you that this is a classic case where the geometry of the part dictates the difficulty of the process. The exhaust valve is trumpet-shaped, with a groove located just below the flared mouth. This groove, with a ring weld diameter of 60 mm, a groove depth of 2 mm, and a fillet radius of 5 mm, is the critical area that requires the wear-resistant cobalt-based alloy deposit. The small diameter and the shallow groove depth mean that the heat input must be carefully controlled to avoid burn-through or excessive dilution, while still achieving a sound metallurgical bond.

The paper reports that prior to 1987, the factory relied on imported Japanese valves because the use of domestic materials resulted in an unacceptably low yield rate. The research goal was to develop a domestic material and process combination that could achieve a yield rate of over 98%, a target that was successfully met. This is a significant achievement, as it demonstrates that with proper process development, domestic materials can match or exceed the performance of imported ones, a lesson I have seen repeated many times in the industry.

Core Technical Points and Process Interpretation

The fundamental challenge in this application is the metallurgical compatibility between the 4Cr10Si2Mo base material and the cobalt-based alloy No. 1 filler wire. 4Cr10Si2Mo is a martensitic stainless steel, typically used for exhaust valves because of its good high-temperature strength and oxidation resistance. Cobalt-based alloy No. 1 (often referred to as Stellite No. 1) is a hard-facing alloy with excellent wear resistance at elevated temperatures, but it has a very different coefficient of thermal expansion and a complex carbide structure.

The key process parameters that the authors likely focused on include the preheat and interpass temperature, the welding current and voltage, the travel speed, and the shielding gas flow rate. For a thin deposit on a small-diameter part, the heat input must be kept low to minimize dilution from the base metal. Excessive dilution would reduce the hardness and wear resistance of the deposit, while too little heat input would result in lack of fusion or porosity.

Parameter Typical Range for TIG Hardfacing Critical Consideration
Preheat Temperature 200-300°C Prevents cracking in the martensitic base material and HAZ.
Interpass Temperature 200-250°C Must be controlled to avoid overheating and grain growth.
Welding Current 80-120 A Low current for thin deposit and small diameter.
Arc Voltage 10-14 V Short arc to minimize heat input and dilution.
Travel Speed 60-100 mm/min Consistent speed ensures uniform deposit thickness.
Shielding Gas Flow 8-12 L/min Argon Adequate shielding prevents oxidation of the cobalt alloy.

The paper mentions that the groove depth is only 2 mm with a radius of 5 mm. This shallow groove means that the deposit must be built up in a single pass or with minimal passes. The fusion line must be clean and free of defects, as any lack of fusion or slag inclusion will serve as a stress raiser and lead to premature failure in service. In my experience, the preparation of the groove is just as important as the welding itself. The groove must be machined to the exact dimensions and cleaned thoroughly to remove any oil, grease, or oxide.

Practical Lessons and Engineering Insights

The achievement of a 98% yield rate is a testament to the importance of systematic process development. In my career, I have seen many cases where a process is "tweaked" on the fly without a clear understanding of the underlying metallurgy, leading to inconsistent results. The authors clearly took a structured approach, likely using a design of experiments or a similar methodology to optimize the process parameters.

One of the critical lessons from this work is the importance of controlling the dilution rate. In hardfacing, the dilution rate is the percentage of the deposit that consists of melted base metal. For cobalt-based alloys, a dilution rate of less than 10% is generally preferred to maintain the desired hardness and corrosion resistance. With a shallow groove, the dilution rate can easily exceed this limit if the welding current is too high or the travel speed is too slow. The authors likely had to carefully balance these parameters to achieve the right dilution.

Another lesson relates to the preheat and post-weld heat treatment. 4Cr10Si2Mo is a martensitic steel that is susceptible to hydrogen-induced cracking. A preheat of 200-300°C is essential to slow the cooling rate and allow hydrogen to diffuse out of the weld zone. After welding, a post-weld heat treatment at a temperature around 700°C may be required to temper the martensite and relieve residual stresses. The paper does not explicitly mention this, but it is a standard practice for this type of steel.

In terms of practical application, this work has significant implications for the marine diesel engine industry. The ability to use domestic materials and processes reduces lead times and costs, and also improves supply chain resilience. I have seen many instances where a factory is forced to shut down production because of a lack of imported components, so this type of import substitution is always welcome.

Study Insights and Implications for the Industry

The success of this project demonstrates that with proper process development, even challenging applications can be brought in-house. The key factors were a clear understanding of the metallurgical requirements, a systematic approach to process optimization, and rigorous quality control to ensure consistency.

For fellow engineers, the takeaway is that the geometry of the part and the required deposit thickness are the primary drivers of the process parameters. Small-diameter parts with thin deposits require low heat input and precise control of the welding variables. The use of a manual TIG process, while labor-intensive, offers the flexibility needed for this type of work. However, for higher volume production, an automated TIG process with a rotating fixture could be considered, as it would provide better consistency and reduce the risk of human error.

In my view, this paper is a valuable reference for anyone involved in the hardfacing of small-diameter components. It highlights the importance of understanding the interaction between the base material, the filler material, and the process parameters. It also serves as a reminder that a high yield rate is not achieved by luck, but by careful planning and execution.