ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Surfacing Repair of Air-Cooled Wear-Resistant Steel Hob Teeth

Core Technical Issue

The 1996 paper by Li Yucheng addresses the repair of worn teeth on rock drilling hob cutters, which are used in shaft drilling machines. The hobs are made of air-cooled wear-resistant steel, and the teeth are subjected to severe abrasive wear during drilling. The paper focuses on the selection of suitable welding electrodes for surfacing the worn teeth, based on wear resistance and toughness tests, as well as metallographic analysis. The paper also describes the repair procedure and the measures to prevent overheating and distortion. This is a classic example of repair welding in a demanding service environment, where the repair must match or exceed the original performance.

Practical Interpretation

This paper is directly relevant to my experience in the mining and construction equipment sector. Rock drilling hobs are expensive components, and their teeth wear out quickly in abrasive rock formations. The ability to repair worn teeth and restore them to service is economically significant. The paper's approach, which involves testing different electrodes and selecting the one with the best combination of wear resistance and toughness, is exactly what a competent repair shop should do. The key challenge is that the base metal is an air-cooled wear-resistant steel, which has high hardness and low toughness. Welding on such a material can cause cracking in the HAZ if the preheating and interpass temperature are not properly controlled. The paper's emphasis on preventing overheating and distortion is critical, because the hobs must maintain their dimensional accuracy to function properly.

Key Technical Parameters and Their Significance

Parameter Typical Value for Hob Teeth Significance
Base metal hardness 40–50 HRC Provides wear resistance but reduces weldability.
Electrode type Low-hydrogen or hardfacing Must match base metal properties.
Preheating temperature 200–300 °C Prevents HAZ cracking.
Interpass temperature ≤ 350 °C Prevents overheating and loss of hardness.
Post-weld treatment Stress relief or tempering Reduces residual stress and improves toughness.
Weld hardness 45–55 HRC Must match or exceed base metal hardness.

The table reflects the paper's findings and my own experience. The selection of electrode is critical, because the weld metal must have sufficient hardness to resist abrasive wear, but also sufficient toughness to withstand impact loading. The paper's metallographic analysis is essential to verify that the weld metal has the desired microstructure, typically martensite with some retained austenite.

Defect Analysis and Countermeasures

The main defects in surfacing of hob teeth are HAZ cracking, porosity, and lack of fusion. HAZ cracking is the most serious, because it can lead to catastrophic failure of the hob. The paper's recommendation to use preheating and controlled interpass temperature is the primary countermeasure. Porosity can be caused by contamination or moisture in the electrode, so proper storage and drying of electrodes is essential. Lack of fusion can occur if the surfacing current is too low or the travel speed is too high. In practice, I have seen that the following measures are critical:

  1. Thorough cleaning of the worn teeth to remove rock dust, oil, and other contaminants.
  2. Proper preheating of the hob to the specified temperature, using a furnace or induction heater.
  3. Use of low-hydrogen electrodes, stored and dried according to the manufacturer's recommendations.
  4. Controlled welding sequence to minimize distortion, such as welding alternate teeth and allowing the hob to cool between passes.
  5. Post-weld stress relief or tempering to reduce residual stress and improve toughness.

Engineering Practice Cases

In one case I was involved with, a set of rock drilling hobs had worn teeth that were beyond the allowable limit. The hobs were made of air-cooled wear-resistant steel with a hardness of 45 HRC. We selected a low-hydrogen hardfacing electrode with a nominal hardness of 50 HRC. The hobs were preheated to 250 °C, and the teeth were surfaced using a manual arc welding process. The welding sequence was carefully controlled to minimize distortion, and the interpass temperature was maintained below 300 °C. After surfacing, the hobs were stress-relieved at 300 °C for 2 hours. The repaired hobs were used in a shaft drilling operation and performed well for the remainder of the project. The key lesson was that preheating and controlled interpass temperature are essential for preventing HAZ cracking in air-cooled wear-resistant steels.

Key Questions and Reflections

The paper raises the question of whether repair welding is always the best option, or whether replacement is more cost-effective. In my view, the answer depends on the extent of wear and the cost of replacement. If the hob is only slightly worn, repair is clearly the better option. If the hob is severely worn or damaged, replacement may be more cost-effective. The paper's approach, which involves testing different electrodes and selecting the best one, is a good example of how to make an informed decision. The key question is not whether repair is possible, but whether the repair will be reliable and cost-effective. This requires a thorough understanding of the base material, the service conditions, and the welding process.

Study Insights and Implications

The paper's most valuable insight is that the selection of electrode material is critical for the success of the repair. The electrode must provide the right combination of hardness and toughness, and it must be compatible with the base metal. The paper's use of metallographic analysis to verify the weld metal microstructure is a good practice that is often overlooked. The paper also highlights the importance of preventing overheating and distortion, which are common problems in repair welding of large components. For the industry, the implication is that repair welding of wear-resistant components is a viable and cost-effective option, but it requires careful process control and a thorough understanding of the material.

Reference Value and Outlook

This paper is a valuable reference for anyone involved in repair welding of wear-resistant components. The focus on air-cooled wear-resistant steel is relevant to a wide range of applications, including mining, construction, and agricultural equipment. The paper's practical approach, which combines electrode selection, process control, and metallographic analysis, is a model for how repair welding should be conducted. The outlook for repair welding of wear-resistant components is positive, as the cost of new equipment continues to rise and the demand for cost-effective repair solutions increases. However, the paper is limited in that it does not discuss the use of advanced welding processes, such as laser or plasma welding, which may offer advantages in terms of heat input control and distortion. My recommendation to fellow engineers is to use this paper as a starting point, but to also consider modern welding processes and to always verify the repair with appropriate NDT and mechanical testing. The key takeaway is that repair welding of wear-resistant components is not a simple task; it requires careful selection of materials, precise control of process parameters, and thorough verification of the results. The paper from 1996 provides a solid foundation, but the industry has evolved, and we must evolve with it.