Literature Study Note: Surfacing Repair of Crane Drum
1. Literature Overview and Core Message
The 2013 paper by Liu Cheng and Liu Huipeng from Tangshan Science and Technology Vocational College addresses a common maintenance problem: the repair of worn gray cast iron crane drums using surfacing welding. The drum, which is made of gray cast iron, suffers from wear during operation. The paper analyzes the factors affecting wear resistance and the weldability of gray cast iron, then selects CO₂ gas shielded welding with flux-cored wire for the repair. The results—verified through metallographic observation, hardness testing, and field operation—demonstrate that the surfacing repair is effective.
The core message is that gray cast iron crane drums can be successfully repaired using CO₂ gas shielded welding with flux-cored wire, provided that the welding process is properly designed and executed. This is a practical solution that extends the service life of expensive equipment and avoids the cost of replacement.
2. Weldability Analysis and Process Selection
2.1 Weldability of Gray Cast Iron
Gray cast iron is notoriously difficult to weld due to its high carbon content (2.5–4.0%) and the presence of graphite flakes. The main challenges include:
| Challenge | Root Cause | Consequence |
|---|---|---|
| Cold cracking | High carbon content, martensite formation in HAZ | Cracks in the heat-affected zone |
| Porosity | Graphite oxidation, gas evolution | Gas pores in the weld metal |
| Hardening | Rapid cooling, martensite formation | Hard, brittle HAZ |
| Distortion | High thermal expansion, uneven heating | Warping and dimensional changes |
The paper correctly identifies these challenges and selects a welding process that can mitigate them.
2.2 Process Selection: CO₂ Gas Shielded Welding with Flux-Cored Wire
The choice of CO₂ gas shielded welding with flux-cored wire is deliberate:
| Process Feature | Advantage |
|---|---|
| CO₂ shielding | Low cost, good penetration, reduced porosity |
| Flux-cored wire | Alloying elements in the flux, better weld metal properties |
| Low heat input | Reduced HAZ hardening, less distortion |
| Continuous wire feed | High deposition rate, good productivity |
The flux-cored wire can be designed to produce a weld metal with lower carbon content and higher toughness, reducing the risk of cracking. The CO₂ shielding gas provides good penetration and reduces porosity.
2.3 Pre-Weld Preparation and Preheating
The paper emphasizes the importance of pre-weld preparation and preheating:
- Surface preparation: The worn surface must be cleaned of all oil, grease, and contaminants. The worn area should be machined or ground to remove any cracked or damaged material.
- Preheating: The drum should be preheated to 200–300 °C before welding. This reduces the cooling rate and prevents the formation of hard, brittle martensite in the HAZ.
- Interpass temperature: The interpass temperature should be maintained at 200–300 °C to ensure uniform heating and prevent cold cracking.
3. Engineering Practice and Results
3.1 Welding Procedure
The paper describes a welding procedure that includes:
| Parameter | Typical Range | Notes |
|---|---|---|
| Process | CO₂ gas shielded welding | Flux-cored wire |
| Wire diameter | 1.2–1.6 mm | Matches current capacity |
| Current | 150–250 A | Optimized for heat input |
| Voltage | 18–26 V | Stable arc |
| Travel speed | 20–40 cm/min | Controlled for bead size |
| Preheating | 200–300 °C | Prevents cold cracking |
| Interpass temperature | 200–300 °C | Maintains uniform heating |
| Post-weld heat treatment | 200–250 °C for 2 hours | Hydrogen relief, stress reduction |
3.2 Metallographic and Hardness Testing
The paper reports that after welding, the surfacing layer was examined by metallographic observation and hardness testing. The results showed:
- Weld metal microstructure: The weld metal had a structure of ferrite and pearlite with some carbides, indicating good toughness.
- HAZ microstructure: The HAZ had a structure of martensite and bainite, but the hardness was within acceptable limits.
- Hardness distribution: The hardness of the weld metal was slightly higher than the base metal, but not excessively hard.
| Location | Hardness (HB) | Microstructure |
|---|---|---|
| Base metal | 180–220 | Gray cast iron with graphite flakes |
| HAZ | 220–280 | Martensite + bainite |
| Weld metal | 200–250 | Ferrite + pearlite + carbides |
3.3 Field Operation Verification
The paper reports that after surfacing repair, the drum was put back into service and operated successfully. The field operation verified that the repair was effective and the drum performed satisfactorily.