ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Hardfacing Repair of Crusher Grate Plates: A Practical Approach

Background and Service Conditions

The 1991 paper by Huang Taiming from Chongqing Iron and Steel's repair department addresses a problem that is all too familiar in the mining and steel industry: the premature wear of crusher grate plates. The F1500×2520 fully water-cooled single-roll crusher used in the sintering plant operates with hot ore particles at approximately 750°C. The grate plates, which are subject to high-temperature abrasive impact, wear out in less than one year of service. The high-temperature wear-resistant alloy layer on the working surface is severely eroded, and the plates must be either replaced or repaired.

From my experience in the steel pipe and fitting industry, I have seen similar wear problems in equipment such as pipe bending dies, roll forming rolls, and guide plates. The economic decision between replacement and repair is always a question of cost, downtime, and the availability of spare parts. In the case of the crusher grate plates, the cost of a new plate is high, and the delivery time is long, so repair by hardfacing becomes an attractive option.

Technical Analysis of the Hardfacing Repair

The repair procedure involves removing the worn hardfacing layer, inspecting the base metal for cracks, and then depositing a new wear-resistant layer using an appropriate hardfacing process. The key technical points are:

  1. Base metal preparation. The worn surface must be ground or machined to sound metal. Any cracks in the base metal must be removed by grinding, otherwise they will propagate during hardfacing.
  2. Hardfacing alloy selection. For high-temperature abrasive wear at 750°C, the hardfacing alloy must maintain hot hardness. Cobalt-based alloys (e.g., Stellite 6 or 12) are suitable, but they are expensive. Iron-based alloys with high chromium content (e.g., Cr-Mo-W alloys) can be used if the temperature is not too high. The paper does not specify the alloy, but the practical choice is a high-chromium iron-based alloy or a cobalt-based alloy.
  3. Preheating and interpass temperature. The base metal of the grate plate is likely a low-alloy steel or cast steel. Preheating to 200–300°C is required to prevent cracking. The interpass temperature must be controlled to avoid overheating and grain growth.
  4. Deposition technique. The hardfacing can be applied by manual metal arc welding (SMAW) with a covered electrode, or by flux-cored arc welding (FCAW) with a self-shielded wire. For large areas, submerged arc welding (SAW) can be used, but it is less common for repair work.

The following table summarizes the typical hardfacing parameters for crusher grate plates:

Parameter Value Comment
Preheat temperature 200–300°C Prevents cracking in the base metal
Interpass temperature 300–400°C Avoids excessive heat input
Welding current 250–350 A (SMAW) Depends on electrode diameter
Arc voltage 25–30 V For SMAW
Travel speed 150–250 mm/min For a 4–5 mm thick deposit
Deposit thickness 5–8 mm Restored to original dimension plus machining allowance
Post-weld cooling Slow cooling in insulating material Prevents stress cracking

Practical Considerations and Lessons Learned

In my experience, the most common mistake in hardfacing repair is insufficient preheating. The base metal, especially if it is cast steel, has a high carbon equivalent, and rapid cooling after welding produces hard, brittle martensite in the heat-affected zone. This leads to cracking, which can occur immediately after welding or during service.

Another critical point is the dilution of the hardfacing alloy with the base metal. If the welding current is too high, or if the electrode is manipulated incorrectly, the base metal melts excessively and dilutes the hardfacing layer. This reduces the hardness and wear resistance of the deposit. The solution is to use a low current and a weaving technique that deposits a thin layer, followed by subsequent passes to build up the required thickness.

The economic benefit of repair is substantial. A new grate plate might cost several thousand dollars, while the repair cost is typically 30–50% of that, plus the downtime for the crusher. In the case described, the repair allowed the crusher to operate for another year, which is a significant saving for the plant.

Summary and Reflection

The hardfacing repair of crusher grate plates is a proven and cost-effective solution for high-temperature abrasive wear. The key to success is a well-designed repair procedure that includes proper base metal preparation, preheating, controlled interpass temperature, and the correct hardfacing alloy. In my years in the industry, I have learned that repair welding is often more demanding than new fabrication because the base metal is already degraded and the repair must restore not only the dimensions but also the mechanical properties. This paper serves as a practical guide for any engineer facing similar wear problems in high-temperature service. The lesson is clear: with proper procedure and process control, a worn component can be returned to service at a fraction of the cost of replacement.