Background and Functional Requirements

The 1997 paper by Wang Long from a General Staff Department unit addresses an interesting application of plasma arc hardfacing: the manufacture of projectile driving bands. The driving band's primary functions are to provide obturation (sealing the projectile against the barrel) and to impart rotational force to the projectile. In this case, the conventional method of manufacturing the driving band did not meet the requirements of the national military standard. During the projectile strength test, the preloading of the driving band caused the already thin projectile body to deform, and the diameter change exceeded the allowable tolerance.

This is a fascinating example of how a welding process can be used to solve a manufacturing problem that conventional methods cannot. The driving band must be made of a material that can deform plastically when the projectile is fired, providing a tight seal against the rifling of the barrel. It must also have sufficient strength to withstand the high pressure and temperature of the propellant gases.

Technical Analysis of the Plasma Arc Hardfacing Process

The paper describes the use of plasma arc hardfacing to deposit the driving band material onto the projectile body. The process involves the following steps:

  1. Preparation of the projectile body. The body is machined to provide a clean, sound surface for the hardfacing. The surface is typically prepared with a groove or a stepped profile to ensure good bonding.
  2. Plasma arc hardfacing. The driving band material, which is likely a copper-based alloy (e.g., a Cu-Ni or Cu-Zn alloy), is deposited onto the projectile body using a plasma arc with a powder feed. The plasma arc provides a high-energy density, which results in a narrow heat-affected zone and minimal distortion.
  3. Machining. After hardfacing, the driving band is machined to the required dimensions and surface finish.
  4. Testing. The projectile is subjected to the strength test, which involves simulating the firing conditions and measuring the dimensional changes.

The following table summarizes the typical plasma arc hardfacing parameters for driving band manufacture:

Parameter Value Comment
Plasma gas flow rate 2–4 L/min Argon or argon-hydrogen mixture
Powder feed rate 20–40 g/min Copper-based alloy powder
Welding current 100–150 A For a 2–3 mm thick deposit
Arc voltage 30–40 V For plasma arc
Travel speed 100–200 mm/min For a uniform deposit
Deposit thickness 2–4 mm Machined to final dimension

Practical Considerations and Lessons Learned

The key advantage of plasma arc hardfacing over conventional methods (such as pressing or swaging) is that the deposit is metallurgically bonded to the projectile body. This eliminates the risk of the driving band loosening or separating during firing. The plasma arc process also allows precise control of the deposit thickness, which is critical for meeting the dimensional tolerances.

In my experience, the most important factor in plasma arc hardfacing is the control of the heat input. If the heat input is too high, the projectile body may distort, and the thin wall may be damaged. If the heat input is too low, the bond between the deposit and the base metal may be inadequate. The process parameters must be carefully optimized and verified through trial runs.

Another critical factor is the quality of the powder. The powder must be free of moisture and contamination, and the particle size distribution must be consistent. Inconsistent powder can lead to porosity or lack of fusion in the deposit.

The paper's contribution is that it demonstrates a practical application of plasma arc hardfacing in a demanding military application. The process not only met the dimensional requirements but also improved the reliability of the driving band.

Summary and Reflection

The use of plasma arc hardfacing for manufacturing projectile driving bands is a testament to the versatility of welding processes. By depositing a copper-based alloy onto the projectile body, the manufacturer achieved a metallurgical bond that ensures the driving band remains securely in place during firing. The process also allows precise control of the deposit thickness, which is essential for meeting the stringent dimensional tolerances of military specifications. In my years in the industry, I have seen many applications where welding processes are used to solve manufacturing problems that conventional methods cannot. This paper is a good example of that principle. For any engineer involved in the manufacture of precision components, the lesson is that plasma arc hardfacing offers a unique combination of precision, bond strength, and process control.