ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

On-Site Surfacing Welding Repair of Φ1000×400 Roll Press

Literature Overview

This paper by Wang Jiang and colleagues from Futuan Building Materials Co., Ltd., Zhengzhou Research Institute of Mechanical Engineering, and Henan Fifth Construction Company addresses a common problem in cement production: the rapid wear of the roll press rolls. The Φ1000×400 roll press is a key piece of equipment in the cement grinding system, and its rolls are subjected to severe abrasive wear from the clinker and other raw materials.

The paper describes a successful on-site repair of a worn roll press using surfacing welding. The repair was performed without removing the roll press from its foundation, which is a significant practical advantage. The authors describe the welding procedure, the materials used, and the results of the repair.

The paper is short and practical, reflecting the pragmatic approach of a plant engineer solving a specific problem. It is a case study of a successful repair that restored the roll press to service and extended its service life.

Core Technical Points

The Roll Press: Function and Failure Modes

The roll press is a high-pressure grinding device used in cement production. It consists of two counter-rotating rolls that crush the material between them. The rolls are subjected to extremely high pressures and severe abrasive wear.

The failure modes of the roll press rolls are:

  1. Abrasive wear - The clinker and other raw materials are hard and abrasive, causing rapid wear on the roll surface.
  2. Surface fatigue - The high-pressure cyclic loading causes surface fatigue cracking and spalling.
  3. Thermal fatigue - The frictional heating during operation can cause thermal fatigue cracking.
  4. Corrosion - The material being ground may contain corrosive components.

The wear of the roll surface is the most common failure mode. The roll surface develops a pattern of wear that reduces the grinding efficiency and increases the power consumption.

The Repair Procedure

The repair procedure described in the paper is a classic on-site surfacing welding repair. The key steps are:

  1. Surface preparation - The worn surface is cleaned and prepared for welding. This involves removing any loose material, oil, and grease.
  2. Preheating - The roll is preheated to a temperature that prevents cracking during welding.
  3. Surfacing welding - The hardfacing material is applied in multiple passes to build up the worn surface.
  4. Post-weld treatment - The repaired surface is inspected and, if necessary, machined to the correct dimensions.

The authors do not provide detailed parameters, but the general approach is well-established. The key parameters that must be controlled are:

Parameter Recommended Range Critical Considerations
Preheat temperature 150-250°C Prevents cracking due to thermal stress
Interpass temperature 200-300°C Controls the cooling rate and microstructure
Welding current 180-260A Depends on the electrode diameter and position
Welding voltage 22-28V Affects arc stability
Welding speed 20-35 cm/min Controls the bead width and heat input
Electrode diameter 3.2-5.0mm Larger diameter for higher deposition
Heat input 10-20 kJ/cm Controls the dilution and hardness

The Hardfacing Material

The hardfacing material used for roll press roll repair is typically a high-chromium iron-based alloy or a tungsten carbide composite. The choice of material depends on the specific application and the wear conditions.

The typical hardfacing materials for roll press rolls are:

Material Type Hardness (HRC) Wear Resistance Toughness Application
High-chromium iron 55-65 Excellent Fair Clinker grinding
Tungsten carbide composite 60-70 Excellent Poor Severe abrasive wear
Martensitic stainless steel 45-55 Good Good General purpose
Nickel-based alloy 40-50 Good Excellent Corrosive environments

The choice of material is critical. In general, a higher hardness provides better wear resistance, but it also reduces the toughness. The material must be selected to provide the best balance of wear resistance and toughness for the specific application.

Integration with Engineering Practice

The Economics of On-Site Repair

The decision to repair the roll press on-site is a significant economic decision. The alternative is to remove the roll press and send it to a repair shop, which involves:

  1. Dismantling and removal - The roll press must be dismantled and removed from the foundation.
  2. Transportation - The roll press must be transported to the repair shop.
  3. Repair - The repair is performed in a controlled environment.
  4. Transportation back - The repaired roll press must be transported back to the plant.
  5. Reinstallation and commissioning - The roll press must be reinstalled and commissioned.

The on-site repair avoids the transportation and dismantling costs, and it reduces the downtime. However, the on-site repair is more difficult because the welding is performed in the field, where the conditions are less controlled.

The Challenges of On-Site Repair

The on-site repair of a roll press presents several challenges:

  1. Accessibility - The roll press is a large, heavy piece of equipment that is difficult to access.
  2. Position - The roll may be in a horizontal or vertical position, which affects the welding technique.
  3. Environmental conditions - The repair site may be dusty, noisy, or subject to weather conditions.
  4. Quality control - The quality of the repair must be verified on-site, which is more difficult than in a repair shop.

The authors do not discuss these challenges in detail, but they are important considerations for any on-site repair.

The Importance of Surface Preparation

The surface preparation is a critical step in the repair process. The worn surface must be clean and free of any contamination. The surface should be ground or machined to remove any cracked or damaged material.

In practice, the surface preparation is often overlooked or performed poorly. This can lead to poor adhesion of the hardfacing layer and premature failure.

The Role of Preheating

Preheating is essential for preventing cracking in the hardfacing layer and the heat-affected zone. The preheat temperature must be carefully controlled to ensure that the cooling rate is slow enough to prevent the formation of martensite in the base metal.

The preheat temperature depends on the material of the roll and the hardfacing material. For a high-chromium iron hardfacing on a carbon steel roll, a preheat temperature of 150-250°C is typically sufficient.

Post-Weld Inspection and Machining