Microstructure and Mechanical Properties of MIG Welded 7020 Aluminum Alloy Joints

Overview and Why This Matters

7020 aluminum is a high-strength Al-Zn-Mg alloy used in structural applications where weight is critical, such as aerospace and military vehicles. Welding it is challenging because the heat of welding degrades the properties in the HAZ. This paper by Peng Xiaoyan et al. provides a detailed characterization of the microstructure and mechanical properties of MIG welded 7020 alloy, using ER5356 filler wire. The findings are directly relevant to anyone who has to weld this alloy and understand why the joint is the weakest link.

Technical Interpretation of the Study

The authors welded 7020 aluminum thick plates using MIG with ER5356 filler wire. The joint properties and microstructure are summarized below.

Property Value Comment
Tensile strength 268 MPa Joint
Yield strength 231 MPa Joint
Elongation 4.5% Joint
Joint efficiency ~0.7 Relative to base metal
Weld zone structure Dendritic cast Coarse grains
Fusion zone structure Columnar near weld, equiaxed near HAZ Transition zone
HAZ structure Partially recrystallized fiber Softened zone
Base metal structure Fiber Rolled
Softening location ~30 mm from weld center Hardness minimum

The joint efficiency of 0.7 is typical for 7020 aluminum welded with ER5356. The weld zone is a dendritic cast structure, which is inherently weaker than the wrought base metal. The fusion zone shows a transition from columnar grains (near the weld) to equiaxed grains (near the HAZ). The HAZ is partially recrystallized, which means that the original fiber structure has been modified by the welding thermal cycle.

The most important finding is the softening zone in the HAZ, located about 30 mm from the weld center. This is caused by coarsening of the η' (MgZn2) precipitates. In the peak-aged condition, 7020 alloy contains fine η' precipitates that provide the main strengthening. When the HAZ is heated during welding, these precipitates coarsen, reducing their effectiveness. The result is a local hardness minimum and a potential weak point in the joint.

Shop Floor and Engineering Practice

This is a classic problem with Al-Zn-Mg alloys. The welding heat input must be carefully controlled to minimize the extent of the HAZ and the degree of over-aging. The 30 mm softening zone is significant. In a thick plate, this zone may be wide enough to affect the overall joint strength.

The choice of ER5356 filler wire is interesting. ER5356 is an Al-Mg alloy, which is commonly used for welding 5xxx and 6xxx alloys. It provides good ductility and corrosion resistance. However, it does not contain zinc, so it cannot be age-hardened. The weld metal will be in the as-welded condition, with a dendritic cast structure.

For 7020 alloy, a better choice might be an Al-Zn-Mg filler, such as ER5183 or a specialized 7xxx filler. These would provide higher strength in the weld metal, but they are more difficult to weld due to their higher hot cracking susceptibility. The authors chose ER5356, which is a compromise between weldability and strength.

In practice, the welding of 7020 requires careful attention to joint preparation, pre-cleaning, and heat input control. The softening zone is inherent to the material and cannot be completely eliminated. However, it can be minimized by using a low heat input process, such as pulsed MIG, and by using a multi-pass technique to reduce the thermal cycle.

Key Questions and Reflections

  1. Can the softening zone be reduced? The softening is caused by precipitate coarsening. A lower heat input would reduce the peak temperature in the HAZ and the time at temperature. This would limit the coarsening. Pulsed MIG or even laser welding could be beneficial.
  2. What is the effect of post-weld heat treatment? If the joint is solution treated and aged after welding, the HAZ precipitates can be re-dissolved and re-precipitated. This could restore the hardness, but it would also affect the weld metal structure. Post-weld aging at a lower temperature might partially restore the HAZ properties without affecting the weld metal.
  3. Is the 0.7 joint efficiency acceptable? For many structural applications, a joint efficiency of 0.7 is the design limit. The joint is designed assuming a reduced strength. If the actual joint efficiency is lower, the structure could fail. It is important to verify the joint efficiency for the specific welding procedure used.
  4. What about corrosion resistance? The HAZ is often the most susceptible to corrosion in aluminum alloys. The precipitate coarsening can lead to a more anodic region, promoting localized corrosion. This is a concern for marine or industrial environments.

Concluding Summary

This paper provides a thorough characterization of the microstructure and mechanical properties of MIG welded 7020 aluminum alloy. The key finding is that the joint efficiency is about 0.7, and the weakest point is the HAZ, where η' precipitates coarsen and cause softening. This is a fundamental limitation of welding this alloy. For engineers designing with 7020, this means that the joint strength must be derated, and the HAZ must be considered in the design. The choice of ER5356 filler provides a good balance of weldability and strength, but it does not eliminate the HAZ softening. To improve the joint performance, a lower heat input process and possibly post-weld aging should be considered. This study is a valuable reference for anyone working with high-strength aluminum alloys.