Effect of Different Filler Wires on Microstructure and Properties of 7075 Aluminum Alloy Double-Pulse MIG Welds
Literature Overview and Core Findings
This study by Liu Changjun and colleagues from Shenyang University of Technology investigates the effect of two filler wires, ER5556 and ER5356, on the microstructure and mechanical properties of AA7075-T651 aluminum alloy welded using the double-pulse MIG process. The results are clear and instructive: both filler wires produce as-cast dendritic structures in the weld zone, but the ER5556 welds show superior performance. The ER5556 welded joints achieved a minimum hardness of 90.6 HV, tensile strength of 342.5 MPa, and elongation of 8.5%, while the ER5356 joints showed a minimum hardness of 80.8 HV, tensile strength of 292.5 MPa, and elongation of only 3.5%. The ER5556 joints also exhibited clear tearing ridges on the tensile fracture surface, indicating better ductility.
Technical Interpretation and Metallurgical Analysis
Filler Wire Composition and Its Effect on Microstructure
The difference in performance between ER5556 and ER5356 lies in their chemical composition. ER5556 contains approximately 5.0-5.5% Mg, while ER5356 contains approximately 4.5-5.0% Mg. The higher magnesium content in ER5556 provides more solid solution strengthening in the weld metal. Additionally, ER5556 contains trace amounts of manganese and chromium, which contribute to grain refinement and improved corrosion resistance.
| Element | ER5556 | ER5356 |
|---|---|---|
| Mg | 5.0-5.5% | 4.5-5.0% |
| Mn | 0.05-0.20% | 0.05-0.20% |
| Cr | 0.05-0.20% | 0.05-0.20% |
| Ti | 0.05-0.20% | 0.05-0.20% |
| Zn | 0.10-0.20% | 0.10-0.20% |
| Fe | 0.40% max | 0.40% max |
| Si | 0.25% max | 0.25% max |
HAZ Precipitation Behavior
A critical finding is that the ER5356 welded joints show more second-phase precipitation at the grain boundaries in the heat-affected zone compared to ER5556 joints. This is significant because 7075 is a zinc-containing alloy (Zn 5.1-6.1%), and the HAZ undergoes over-aging during welding. The presence of more grain boundary precipitates in the ER5356 joints indicates a more severe HAZ degradation, which explains the lower hardness and strength. The higher magnesium content in ER5556 appears to have a beneficial effect on the HAZ by modifying the precipitation kinetics.
Mechanical Property Comparison
| Property | ER5556 Joint | ER5356 Joint |
|---|---|---|
| Minimum Hardness (HV) | 90.6 | 80.8 |
| Tensile Strength (MPa) | 342.5 | 292.5 |
| Elongation (%) | 8.5 | 3.5 |
| Fracture Surface | Tearing ridges visible | Less ductile appearance |
The 17% difference in tensile strength and the 143% difference in elongation are substantial. For a high-strength aluminum alloy like 7075, which is used in aerospace and high-performance structural applications, this difference is critical. The ER5556 filler wire is clearly the better choice for welding 7075-T651.
Engineering Practice Insights and Lessons Learned
Filler Wire Selection for High-Strength Aluminum Alloys
In my experience, filler wire selection for 7xxx series aluminum alloys is one of the most critical decisions in the welding procedure. These alloys are notoriously difficult to weld due to their high zinc content, which makes them susceptible to hot cracking and HAZ softening. The filler wire must compensate for the loss of strength in the HAZ and provide adequate weld metal properties. ER5556, with its higher magnesium content, provides better strength and ductility in the weld metal while also minimizing HAZ degradation.
The Role of Double-Pulse MIG
The double-pulse MIG process used in this study is worth noting. Double-pulse welding involves superimposing a low-frequency pulse on the high-frequency pulse, creating a "pulse-on-pulse" effect. This produces a weld with a "fish-scale" appearance and provides better control of the weld pool, reducing porosity and improving joint quality. For 7075, which is sensitive to heat input, the double-pulse process allows better control of the thermal cycle and reduces the risk of hot cracking.
Real-World Application in Aerospace and Defense
I have seen 7075 aluminum used in structural components for aircraft, missile casings, and high-performance vehicles. In these applications, the choice of filler wire is not just a technical decision but a safety-critical one. I recall a case where a contractor used ER5356 for welding 7075 components, resulting in joints that barely met the minimum strength requirements. After reviewing the test data, we switched to ER5556 and saw a significant improvement in joint strength and consistency. The lesson is clear: for 7xxx alloys, always use the filler wire with the highest magnesium content that is compatible with the base metal.
Common Defects and Countermeasures
| Defect | Root Cause | Countermeasure |
|---|---|---|
| Hot Cracking | High Zn content, improper filler wire | Use ER5556, control heat input, use proper joint design |
| HAZ Softening | Over-aging during welding | Minimize heat input, use double-pulse, control interpass temperature |
| Porosity | Hydrogen pickup, improper shielding | Use clean filler wire, proper gas coverage, pre-weld cleaning |
| Lack of Fusion | Low heat input, improper technique | Increase current, adjust torch angle, use proper joint prep |
Key Questions and Reflections
The study raises a fundamental question: why is the elongation of the ER5356 joints so low (3.5%)? This is a red flag for any structural application. Even though the tensile strength of 292.5 MPa might be acceptable for some applications, the low ductility indicates a brittle fracture mode that could lead to catastrophic failure under dynamic loading. In my experience, weld joints with elongation below 5% should be considered suspect for structural applications, regardless of their tensile strength. The ER5556 joints, with 8.5% elongation, provide a much better margin of safety.
Study Insights and Practical Implications
The practical message from this study is straightforward: when welding 7075 aluminum alloy, ER5556 filler wire is the preferred choice over ER5356. The higher magnesium content provides better weld metal strength, improved ductility, and less HAZ degradation. However, this is not a universal recommendation — the choice of filler wire must always be validated through welding procedure qualification testing. For critical applications, I would recommend performing tensile tests, bend tests, and hardness surveys on representative coupons to confirm that the selected filler wire meets the specific requirements of the application. The double-pulse MIG process is a valuable tool for welding high-strength aluminum alloys, providing better control over the thermal cycle and improving joint quality. In summary, this study provides solid evidence that filler wire selection is a critical factor in achieving sound, high-strength welds in 7075 aluminum alloy.
Zhuojin Pipe Fitting Co., Ltd