ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Microstructure Analysis of AZ31B Magnesium Alloy TIG-MIG Double Arc Welding

Literature Overview and Process Context

This paper by Ping Qiwen, Ma Guohong, Hu Xiaowu, and Ye Jia from Nanchang University and the University of Kentucky, published in Hot Working Technology (热加工工艺), Volume 44, Issue 3, 2015, pages 196-198, addresses a topic that is increasingly important in the automotive and aerospace industries: welding of magnesium alloys. The material is AZ31B, a 2 mm thick sheet, and the process is TIG-MIG double arc welding. The funding from the National Natural Science Foundation (61165008) and the Jiangxi Provincial Natural Science Foundation (20114BAB206004) indicates that this is a research area with significant government support, and rightly so, because magnesium alloys are lightweight and have good specific strength, but they are difficult to weld. The authors have used optical microscopy and SEM to analyze the joint microstructure and the phase composition, and they have identified the key features that determine the mechanical properties. This is a practical paper that tells you what to expect when you weld AZ31B and where the problems are likely to occur.

Joint Microstructure and Fusion Zone Characteristics

The authors report that the joint consists of three zones: base metal, heat-affected zone (HAZ), and weld metal, with a distinct fusion zone between the HAZ and the weld metal. The fusion zone is formed from the semi-molten state at the pool boundary, and it is the region where the base metal is partially melted and then solidified. This is a critical region because it is where the base metal grains are partially melted, and the liquid film that forms at the grain boundaries can lead to liquation cracking. The authors note that the fusion zone has a high concentration of precipitates, specifically Mg17Al12, which is the main intermetallic phase in the Mg-Al system. This is a significant observation because Mg17Al12 is brittle and has a low melting point, so its presence at the grain boundaries in the fusion zone will reduce the ductility and the strength of the joint. The weld metal has a finer grain structure than the base metal, which is a result of the rapid solidification in the weld pool, but it also contains multiple intermetallic compounds, which can be either beneficial or detrimental depending on their size and distribution.

Zone Microstructure Key Feature Mechanical Implication
Base metal α-Mg solid solution Equiaxed grains Good ductility
HAZ α-Mg + Mg17Al12 Precipitate coarsening Reduced ductility
Fusion zone Semi-molten, partially melted grains Mg17Al12 at grain boundaries Poor mechanical properties, liquation cracking risk
Weld metal Fine α-Mg grains Multiple intermetallic compounds Variable, depends on precipitate size and distribution

Precipitate Analysis and Mechanical Implications

The authors report that the fusion zone has a high concentration of Mg17Al12 precipitates, and they infer that this region has poor mechanical properties. This is a reasonable inference, because Mg17Al12 is a hard and brittle phase, and its presence at the grain boundaries will reduce the ductility and the toughness of the joint. The weld metal also contains multiple intermetallic compounds, but the authors do not identify them specifically. In the Mg-Al system, the main intermetallic compounds are Mg17Al12 and Mg2Al3, and both can form during welding. The presence of these compounds in the weld metal is not necessarily a defect, because they can act as strengthening phases if they are small and uniformly distributed. However, if they are large and concentrated at the grain boundaries, they will reduce the ductility and the fatigue life. The authors have identified the fusion zone as the critical region, and this is consistent with my experience: in magnesium alloy welds, the fusion zone is often the weakest link, and it is where cracks initiate under load.

Engineering Practice Implications and Key Lessons

This paper is a useful reference for anyone welding AZ31B magnesium alloy, and it has several practical implications. First, the fusion zone is the critical region, and it is where the mechanical properties are poorest. This means that the joint strength will be governed by the fusion zone, not by the weld metal or the base metal. Second, the Mg17Al12 precipitates at the grain boundaries in the fusion zone are the cause of the poor mechanical properties, and they are formed during solidification. A faster cooling rate will reduce the amount of Mg17Al12 that forms, but it may also increase the risk of cracking. Third, the TIG-MIG double arc process is a viable method for welding thin magnesium sheets, but it requires careful control of the heat input to avoid excessive grain growth and excessive precipitation. The practical lesson is to use a low heat input and a high travel speed to minimize the fusion zone width and the amount of Mg17Al12 that forms. In my experience, magnesium alloy welding is unforgiving, and the best results come from a process that is tuned to the specific alloy and thickness. The paper is a solid contribution to the literature, and I would recommend it to any engineer who is welding magnesium alloys for structural applications. The next step would be to investigate the effect of the TIG-MIG arc ratio on the joint properties, because the current study does not address that variable in detail, and it is critical for process optimization.