TA2 Titanium/1060 Aluminum Dissimilar Metal Pulse MIG Brazing

Literature Overview and Core Findings

This study by Wei Shouzheng et al. from North University of China and Beijing Aeronautical Manufacturing Technology Research Institute, published in 2018, addresses one of the most challenging dissimilar metal joints: titanium to aluminum. The paper uses Al-Si filler wire to join TA2 titanium to 1060 aluminum in a butt joint configuration using pulse MIG (P-MIG) brazing. The joint microstructure is analyzed using SEM and EDS, and the joint reliability is evaluated using tensile testing and fracture surface analysis.

The core finding is that a reliable TA2/1060Al MIG brazed joint can be achieved with good process stability and repeatability. The titanium and the weld are joined by brazing through a bud-like Ti(Al,Si)3 intermetallic compound layer with a thickness of 1-5 μm. In tensile testing, all Ti/Al MIG brazed joints fracture in the aluminum base metal, indicating that the brazing interface bond strength exceeds the aluminum base metal strength.

This is a significant paper for anyone involved in joining titanium to aluminum, which is a critical challenge in aerospace, chemical processing, and marine applications. Titanium and aluminum are metallurgically incompatible: they form brittle intermetallic compounds (TiAl, TiAl2, TiAl3, Ti3Al) when they are melted together, and they have very different melting points (1668°C vs. 660°C) and coefficients of thermal expansion (8.6 μm/m·K vs. 23.1 μm/m·K). The MIG brazing process addresses this by melting only the aluminum filler wire, not the titanium base metal, so that the titanium remains solid and the joint is formed by brazing.

Technical Interpretation: The Ti(Al,Si)3 Intermetallic Layer

The paper reports that the titanium and the weld are joined by brazing through a bud-like Ti(Al,Si)3 intermetallic compound layer with a thickness of 1-5 μm. This is a critical finding because the IMC layer thickness determines the joint strength. If the IMC layer is too thin, the bond may be weak; if it is too thick, the IMC is brittle and the joint may fail at the interface.

The presence of silicon in the filler wire is important. The Al-Si filler wire (likely ER4043 or ER4047) contains 5-12% silicon. The silicon reacts with the titanium to form Ti(Al,Si)3, which is a ternary intermetallic compound that is less brittle than the binary TiAl3. The silicon also promotes wetting of the titanium by the aluminum filler wire, which is essential for brazing.

The bud-like morphology of the IMC layer is interesting. It suggests that the IMC grows preferentially at certain locations on the titanium surface, possibly at grain boundaries or other high-energy sites. This is consistent with the known growth mechanism of IMCs in dissimilar metal brazing.

The tensile test results are the most important finding. All joints fracture in the aluminum base metal, which means that the brazing interface bond strength exceeds the aluminum base metal strength. This is the ideal outcome for a dissimilar metal joint: the joint fails in the weaker base metal rather than at the interface. The paper reports that the Ti/Al MIG brazed joints have good process stability and repeatability, which is essential for production applications.

Engineering Practice: What This Means on the Shop Floor

Parameter Ti/Al MIG Brazed Joint