ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Narrow-Gap TIG Welding of Q235 Steel: Microstructure, Mechanical Properties, and Corrosion Behavior

Literature Overview and Practical Significance

This study from Beijing Institute of Petrochemical Technology examines narrow-gap TIG welding of Q235 thick-wall pipe using a deep U-groove. Q235 is a common structural carbon steel, but the relevance here is the narrow-gap technique itself. For thick-wall pipe, the traditional approach is to use a V-groove or U-groove with multiple passes, which consumes a lot of filler metal and generates a lot of heat. Narrow-gap welding reduces the groove volume, which reduces the number of passes, the heat input, and the residual stress. The paper shows that the resulting joint has good tensile strength, good elongation, and acceptable impact toughness, but the corrosion resistance of the heat-affected zone is compromised. This is a critical finding because in many applications, the pipe is in contact with a corrosive medium, and the HAZ is often the first place to fail.

Key Technical Points and Process Windows

Joint Geometry and Welding Parameters

The paper uses a deep U-groove, which is the standard geometry for narrow-gap welding. The key parameters are the groove width, the root face, and the welding current. In narrow-gap TIG, the torch must fit into the groove, so the groove width is typically 8 to 12 mm at the top, tapering to a root gap of 3 to 4 mm. The welding current is lower than in conventional TIG because the heat input must be carefully controlled to avoid sidewall fusion defects. The paper reports an average tensile strength of 450 MPa, which is close to the base metal strength of Q235. The elongation is 26.3%, which is good for a welded joint. The impact energy in the weld zone is 91.1 J, which is excellent, but the HAZ impact energy is only 60.1 J, which is still acceptable but noticeably lower.

Microstructural Analysis

The weld zone shows recrystallization and the formation of fine equiaxed grains. This is a result of the thermal cycle in the weld pool, which promotes grain refinement. The fine grains increase both hardness and tensile strength. The HAZ, however, shows coarse ferrite and pearlite. This is the typical coarse-grained heat-affected zone (CGHAZ) that forms near the fusion line where the peak temperature is high and the cooling rate is slow. The coarse grains are a result of grain growth during the welding thermal cycle. The paper notes that the material uniformity in the HAZ is destroyed, which leads to a significant reduction in corrosion resistance.

Corrosion Behavior

The electrochemical tests show that the corrosion resistance of the HAZ is lower than that of the weld zone and the base metal. This is a direct consequence of the microstructural heterogeneity. The coarse grains in the HAZ create more grain boundaries, which act as preferential sites for corrosion. The potential difference between the coarse-grained HAZ and the fine-grained weld zone creates a galvanic couple, which accelerates corrosion. This is a classic problem in welded carbon steel pipe, and it is one of the reasons why we specify post-weld heat treatment or stress relief for critical service.

Zone Microstructure Impact Energy (J) Corrosion Resistance
Weld Zone Fine equiaxed grains 91.1 Higher
HAZ Coarse ferrite and pearlite 60.1 Lower
Base Metal Ferrite and pearlite - Baseline

Engineering Practice and Shop Floor Insights

I have seen the consequences of ignoring HAZ corrosion in carbon steel pipe. In one project, we had a water injection line that failed after only two years of service. The failure was located exactly at the HAZ of a girth weld. The pipe was Q235, and the welding procedure had not specified any post-weld heat treatment. The HAZ had a coarse microstructure, and the corrosion rate was significantly higher than in the base metal. The failure was a pinhole leak that eventually grew into a full rupture. The cost of the repair, including the shutdown, was several times the cost of the original pipe.

The paper's finding that the HAZ corrosion resistance is lower than the weld zone and base metal is a warning to every engineer who specifies carbon steel pipe for corrosive service. If the pipe is going to carry a corrosive medium, you need to consider the HAZ as a weak link. The options are to use a corrosion-resistant alloy, to apply a coating, or to specify a post-weld heat treatment that refines the HAZ grains. The paper does not address the effect of PWHT on the HAZ, but I know from experience that a stress relief at 600°C to 650°C can partially refine the coarse grains and improve the corrosion resistance.

Key Questions and Reflections

The paper reports a tensile strength of 450 MPa, but the base metal Q235 has a minimum yield strength of 235 MPa and a tensile strength range of 370 to 500 MPa. The joint strength is at the lower end of the base metal range, which means the joint efficiency is around 90% to 100%. This is acceptable for most applications, but it is worth noting that the weld metal is not overmatched. In a high-strength application, you would want the weld metal to be stronger than the base metal to ensure that failure occurs in the base metal, not in the weld. For Q235, the weld metal strength is adequate, but for higher strength steels, narrow-gap TIG may not be the best choice.

The paper does not discuss the effect of welding position. Narrow-gap TIG is typically performed in the flat position because the torch and wire feed are oriented vertically. For girth welds on pipe, the welding is often done in the 5G position, which means the pipe is horizontal and the weld is made in the vertical and overhead positions. Narrow-gap TIG in the vertical position is difficult because the molten pool tends to sag. This is a practical limitation that the paper does not address.

Study Insights and Implications

The key insight from this paper is that narrow-gap TIG produces a sound joint with good mechanical properties, but the HAZ is a weak point in terms of corrosion resistance. This is a fundamental metallurgical issue that cannot be avoided by changing the welding parameters alone. The HAZ will always have a coarser microstructure than the weld zone because of the thermal cycle. The only way to mitigate the problem is to control the heat input, use a lower interpass temperature, or apply a post-weld heat treatment.

For the shop floor, the practical implication is that narrow-gap TIG is a viable process for thick-wall Q235 pipe, but you must not ignore the HAZ. If the pipe is for corrosive service, you need to specify a PWHT or a corrosion-resistant coating. If the pipe is for non-corrosive service, the HAZ is less of a concern, but you still need to ensure that the impact toughness is adequate for the design temperature.

Reference Value and Outlook

This paper provides a useful baseline for narrow-gap TIG welding of carbon steel. The data on mechanical properties and corrosion behavior is valuable for engineers who are considering this process for thick-wall pipe. The finding that the HAZ has lower corrosion resistance is a reminder that welding is not just about strength; it is also about the integrity of the entire joint.

For future work, I would like to see data on the effect of PWHT on the HAZ corrosion resistance. I would also like to see data on the welding of higher strength steels, such as API 5L X65 or X70, where the HAZ is even more critical. Narrow-gap TIG has the potential to reduce welding time and cost, but it must be qualified for the specific service conditions.

In conclusion, this paper is a valuable contribution to the literature on narrow-gap welding. It confirms that the process can produce a sound joint, but it also highlights the HAZ as a weak link in corrosive service. I would recommend this paper to any engineer who is considering narrow-gap TIG for carbon steel pipe, with the caveat that the HAZ must be carefully evaluated for the intended service environment.