ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

AZ91B Magnesium Alloy TIG Welding: Filler Wire Selection and Hot Cracking Control

The Weld Structure and Its Weaknesses

This paper by Xu Jinfeng and Zhai Qiuya at Xi'an University of Technology examines the microstructure and mechanical properties of TIG welded AZ91B magnesium alloy joints using AZ61 and AZ91 filler wires. AZ91B is a common die-casting magnesium alloy, but it is not typically considered a welding-friendly material because of its high aluminium content and the associated hot cracking tendency. The paper provides a detailed analysis of the weld structure and the factors that influence joint quality.

The weld structure is described as consisting of well-developed, snowflake-shaped α-Mg dendrites with a low-melting-point eutectic of α-Mg + Mg17Al12 in the intergranular regions. The fusion zone has a fine equiaxed α-Mg structure with intergranular eutectic, and the heat-affected zone (HAZ) is close to the base metal, with coarse α-Mg dendrites and intergranular eutectic. This structure is typical for magnesium alloys, and it highlights the key weakness: the low-melting-point eutectic in the intergranular regions is a potential site for hot cracking.

The Hot Cracking Mechanism: Why Composition Drift Matters

The paper's most important finding is the mechanism of hot cracking. During welding, magnesium evaporates due to the high arc temperature, which increases the relative aluminium content in the weld pool. This increases the amount of eutectic in the weld metal, which in turn increases the hot cracking tendency. This is a classic composition drift problem, and it is particularly severe in magnesium alloys because magnesium has a high vapour pressure.

The paper reports that using ERAZ61 filler wire gives a joint with better hot cracking resistance and better composition and microstructure consistency with the base metal. This is because AZ61 has a lower aluminium content than AZ91, so the weld metal composition is closer to the base metal after magnesium evaporation. The lower aluminium content also reduces the amount of eutectic, which reduces the hot cracking tendency.

Filler Wire Al Content Eutectic Amount Hot Cracking Tendency Joint Quality
ERAZ61 Lower Lower Lower Better
ERAZ91 Higher Higher Higher Worse

Filler Wire Selection: ERAZ61 vs ERAZ91

The practical lesson from this paper is that filler wire selection is not just about matching the base metal composition — it is about compensating for composition drift during welding. For AZ91B base metal, using ERAZ61 filler wire is the better choice because it compensates for the magnesium evaporation and keeps the weld metal composition closer to the base metal. This reduces the hot cracking tendency and improves joint quality.

I have seen this principle applied in other alloy systems. For example, when welding aluminium alloys, you often use a filler wire with a slightly different composition to compensate for dilution and composition drift. The same principle applies to magnesium alloys, and this paper provides a clear example.

The paper also highlights the importance of controlling the welding parameters to minimise magnesium evaporation. Using a lower heat input, a shorter arc length, and a faster travel speed can all help to reduce evaporation and keep the weld metal composition stable. This is a practical consideration that is often overlooked in production welding.

Key Questions and Reflections

One question that comes to mind is whether the hot cracking tendency can be further reduced by using a filler wire with an even lower aluminium content, such as AZ31. However, this would reduce the strength of the weld metal, so there is a trade-off between hot cracking resistance and mechanical properties. The paper does not investigate this trade-off, which is a gap in the research.

Another reflection: the paper only investigates TIG welding, but magnesium alloys are often welded using other processes, such as laser welding or friction stir welding. The composition drift mechanism may be different for these processes, and the filler wire selection may need to be adjusted accordingly.

Study Insights and Implications

The main insight from this paper is that filler wire selection for magnesium alloys is not just about matching composition — it is about compensating for composition drift during welding. For AZ91B base metal, ERAZ61 filler wire is the better choice because it reduces the hot cracking tendency and improves joint quality.

This has practical implications for welding procedure development. When you are qualifying a welding procedure for AZ91B, you should specify the filler wire type and composition, and you should verify that the weld metal composition is within the specified range after welding. If the weld metal composition is outside the range, you may need to adjust the filler wire or the welding parameters.

Reference Value and Outlook

This paper is a valuable reference for anyone welding AZ91B magnesium alloy. It provides a clear explanation of the hot cracking mechanism and practical guidance on filler wire selection. For future work, I would like to see studies on the effect of welding parameters on composition drift and hot cracking, and studies on the use of alternative welding processes for AZ91B.

The bottom line is that welding AZ91B magnesium alloy requires careful attention to filler wire selection and welding parameters. Using ERAZ61 filler wire and controlling the welding parameters to minimise magnesium evaporation will give you a joint with good hot cracking resistance and acceptable mechanical properties. If you ignore these factors, you will get hot cracking and poor joint quality, which is a recipe for failure in service.