Double-Sided TIG Welding of Cast AZ91D Magnesium Alloy: Microstructural Evolution and Surface Quality

Literature Overview and Welding Procedure

The paper by Guo Qiang, You Guoqiang and Wu Jingting, published in Hot Working Technology in 2011, describes an investigation into the double-sided TIG welding of 3 mm thick cast AZ91D magnesium alloy. The authors used AC TIG welding, with a front-side welding current of 120 A and a back-side welding current of 80, 90 or 100 A. The welding speed and the shielding gas flow rate were kept constant. After welding, the joints were sectioned and examined using optical microscopy. The results showed that the weld surface formation was poor, with visible defects. As the back-side welding current increased, the network-like β-Mg17Al12 phase in the weld decreased, while the granular β-Mg17Al12 phase increased.

From my perspective, this paper addresses a specific problem: the welding of cast magnesium alloys, which are more difficult to weld than wrought alloys due to their coarse-grained structure and the presence of casting defects. The double-sided welding approach is used to reduce the heat input per side and to improve the penetration and the weld quality.

Weld Surface Formation and Defects

The authors reported that the weld surface formation was poor, with visible defects. This is a common problem in magnesium welding, and it can be attributed to several factors:

  1. Oxidation: The magnesium oxide layer on the surface prevents wetting and fusion, leading to an irregular bead shape.
  2. Porosity: The high solubility of hydrogen in molten magnesium causes porosity, which can appear as surface defects.
  3. Undercut: The high heat input can cause the weld pool to spread, leading to undercut at the edges.
  4. Spatter: The AC welding process can cause spatter, which can contaminate the weld.

The double-sided welding approach can help to reduce the heat input per side, but it also introduces a new set of challenges. The back-side weld must be aligned with the front-side weld, and the penetration must be sufficient to fuse the two welds together. If the back-side weld is not aligned, it can cause lack of fusion or a cold lap.

Microstructural Analysis and Phase Transformation

The microstructural analysis revealed that the weld contained a network-like β-Mg17Al12 phase, which is a brittle intermetallic compound. This phase is formed during solidification, and it can reduce the ductility and toughness of the weld. As the back-side welding current increased, the network-like phase decreased, and the granular phase increased. This is an interesting finding, as it suggests that the higher back-side current promotes the formation of a more favorable microstructure.

The transformation from a network-like to a granular phase can be explained by the thermal history of the weld. A higher back-side current increases the heat input, which slows down the cooling rate. This allows the β-phase to coarsen and to become more granular, rather than forming a continuous network. However, a higher heat input can also cause grain growth and the formation of a coarse-grained HAZ, which can reduce the mechanical properties.

The authors did not report the mechanical properties of the welds, which is a limitation. The microstructural analysis is useful, but it does not provide a complete picture of the joint quality. A comprehensive study would include tensile, bend and hardness tests, as well as corrosion testing.

Practical Implications for Cast Magnesium Components

Cast AZ91D magnesium alloy is used in automotive and electronics applications, such as instrument panels, steering wheels and laptop casings. The welding of cast components is challenging due to the presence of porosity and inclusions in the casting. The double-sided welding approach can help to reduce the heat input and to improve the weld quality, but it requires careful control of the welding parameters.

From a practical standpoint, the following considerations are important:

  1. Casting quality: The casting must be free of porosity, inclusions and other defects. A defective casting will produce a defective weld.
  2. Joint preparation: The joint must be prepared carefully, with a clean surface and a uniform gap. The root face should be small, and the groove angle should be appropriate for the material thickness.
  3. Welding parameters: The front-side and back-side currents must be balanced to achieve the desired penetration and weld quality. The welding speed and the shielding gas flow rate must be optimized.
  4. Inspection: The weld must be inspected for porosity, lack of fusion and other defects. Radiography or ultrasonic testing may be required for critical applications.

Conclusion

The paper by Guo et al. provides valuable insights into the double-sided TIG welding of cast AZ91D magnesium alloy. The microstructural analysis shows that the back-side welding current has a significant effect on the formation of the β-Mg17Al12 phase, which is an important factor for the mechanical properties. However, the paper does not report the mechanical properties, which is a limitation. The poor weld surface formation and the presence of defects highlight the challenges of welding cast magnesium alloys. I would recommend that any fabricator working with cast magnesium components conduct a comprehensive qualification program, including mechanical testing and metallurgical analysis, before applying the process in production. The double-sided welding approach has potential, but it requires careful process control and a high-quality casting.