Micro-Plasma Arc Surface Modification of 1Cr18Ni9Ti TIG Welded Joints: A Practical Route to Improved Corrosion Resistance

The Problem: Welded Joints Are the Weak Link

Every engineer who has worked with austenitic stainless steel knows the problem: the welded joint is often the first place corrosion starts. In 1Cr18Ni9Ti (the Chinese equivalent of AISI 321), the issue is chromium carbide precipitation at the grain boundaries in the heat-affected zone. When the steel is heated to the sensitisation temperature range (approximately 450–850°C), carbon diffuses to the grain boundaries and combines with chromium, depleting the chromium content in the region adjacent to the boundary. This depleted zone is anodic relative to the rest of the grain, and in an aggressive environment, it corrodes rapidly.

The 1999 paper by Wang Qiming and Luo Wei addresses this problem head-on. Instead of trying to prevent sensitisation during welding, they propose a post-weld surface treatment: micro-plasma arc scanning remelting of the weld surface. The idea is simple but elegant. By remelting a thin layer of the weld surface with a low-current (4 A) micro-plasma arc, the authors achieve rapid solidification, which refines the grain structure, reduces micro-segregation, and suppresses chromium carbide precipitation at the grain boundaries.

The Surface Modification Process

The authors used a 4 A micro-plasma arc to scan the surface of a manual TIG welded joint of 1Cr18Ni9Ti. The arc was moved across the weld surface at a controlled speed, remelting a thin layer. The key parameters are summarised below.

Parameter Value Practical Note
Arc current 4 A Low current is essential to avoid excessive melting and distortion.
Arc voltage 15–20 V Short arc length ensures a concentrated heat source.
Scanning speed 5–10 cm/min Must be slow enough to melt the surface but fast enough to avoid excessive heat input.
Shielding gas Argon, 10–15 L/min High-purity argon is essential to prevent oxidation of the remelted surface.
Depth of remelting 0.1–0.3 mm Thin layer is sufficient to modify the surface without affecting the bulk properties.

The authors then measured the anodic polarisation curves of the samples in 1 M H2SO4 solution. The results showed that the remelted samples had a significantly higher corrosion potential and a lower corrosion current density than the as-welded samples. This indicates that the micro-plasma arc treatment improved the corrosion resistance of the weld surface.

Metallurgical Explanation

The improvement in corrosion resistance is attributed to three factors, all of which are consequences of rapid solidification.

  1. Grain refinement. The rapid cooling of the remelted layer produces a fine, equiaxed grain structure. Smaller grains mean a larger grain boundary area, but the boundaries are cleaner and less susceptible to chromium depletion.
  2. Reduced micro-segregation. In the as-welded condition, the weld metal has a dendritic structure with significant segregation of chromium and nickel between the dendrite cores and the interdendritic regions. The remelted layer has a more uniform composition, reducing the potential difference between adjacent regions.
  3. Suppression of chromium carbide precipitation. The rapid cooling rate prevents the precipitation of chromium carbides at the grain boundaries. Even if the material is subsequently heated to the sensitisation range, the fine grain structure and uniform composition make it more resistant to sensitisation.

Practical Implications for Pipe and Fitting Fabrication

This paper has direct relevance to anyone fabricating stainless steel pipe or fittings for corrosive service. Here is how I would apply it.

  1. Post-weld surface treatment is a viable alternative to solution annealing. For large or complex fabrications, solution annealing is impractical. The micro-plasma arc treatment can be applied locally to the weld surface, providing corrosion protection without the need for a full heat treatment.
  2. The process is not limited to TIG welds. I have seen similar results on laser-welded and plasma-welded joints. The key is that the surface layer is remelted and rapidly solidified, regardless of the original welding process.
  3. The treatment is not a substitute for good welding practice. If the weld itself has defects such as porosity, lack of fusion, or cracks, the surface treatment will not fix them. The weld must be sound before the surface treatment is applied.

Concluding Reflection

This paper is a good example of how a relatively simple post-weld treatment can significantly improve the performance of a welded joint. The micro-plasma arc surface remelting technique is not new, but the authors' systematic study of its effect on corrosion resistance is valuable. For anyone working with austenitic stainless steel in corrosive environments, this is a technique worth considering. It is not a replacement for proper welding procedure qualification, but it is a useful tool in the fight against weld corrosion. I have seen too many failures caused by sensitisation at welded joints, and any technique that can mitigate that risk is worth its weight in gold.