ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Effect of Activating Flux on Microstructure and Properties of TIG Welded Stainless Steel Joints

Literature Overview and Core Findings

This paper, published in Welding Technology in 2014, investigates the effect of activating fluxes on the TIG welding of stainless steel. The authors tested two different fluxes, designated G1 and G2, and compared the arc shape, weld penetration, weld width, microstructure, and microhardness with those of conventional TIG welding. The results show that with the same welding parameters, the use of activating flux produces a good weld surface and increases the depth-to-width ratio. Flux G1 increased the depth-to-width ratio by 5.5 times compared to conventional TIG, while the microhardness of the fusion zone remained unchanged. Flux G2 produced a more uniform and finer austenite grain structure in the fusion zone, with a slight increase in microhardness and a more uniform distribution. The paper aims to develop an economical and practical activating flux formulation for stainless steel TIG welding.

Technical Interpretation and Metallurgical Analysis

The Principle of A-TIG Welding

Activating TIG (A-TIG) welding is a technique where a thin layer of activating flux is applied to the surface of the workpiece before welding. The flux contains oxides and halides, which have two main effects. First, the flux decomposes in the arc, releasing oxygen and other elements that cause the arc to constrict. The constricted arc has a higher current density, which increases the penetration depth. Second, the flux changes the surface tension of the molten pool, creating a Marangoni flow that directs the molten metal downward, further increasing penetration. The combination of these effects gives a high depth-to-width ratio, which is the primary benefit of A-TIG.

The Effect of Flux Composition

The paper tested two fluxes, G1 and G2. Flux G1 gave a depth-to-width ratio of 5.5 times that of conventional TIG, but no change in microhardness. This suggests that G1 is a strong arc constrictor, but it does not significantly affect the microstructure. Flux G2 gave a smaller increase in depth-to-width ratio, but it produced a finer and more uniform austenite grain structure, with a slight increase in microhardness. This suggests that G2 contains elements that act as grain refiners, such as titanium or aluminum, which form fine oxides or nitrides that nucleate the austenite grains. The difference between the two fluxes is important for practical applications. If you need maximum penetration, use G1. If you need a better microstructure, use G2.

Microstructure and Microhardness

The paper reports that the fusion zone of the A-TIG weld has a finer grain structure than conventional TIG. This is because the arc constriction reduces the heat input per unit length, and the weld pool solidifies faster. The faster cooling rate gives a finer grain size. The microhardness of the fusion zone is slightly higher with G2, which is consistent with the finer grain size. However, the microhardness of the heat-affected zone (HAZ) is not significantly different. This is important because a coarse HAZ can be a weak point in a weld. The paper shows that A-TIG does not worsen the HAZ.

Integration with Engineering Practice

Application to Stainless Steel Pipe Welding

In our industry, A-TIG is particularly useful for welding stainless steel pipes, especially in the food, pharmaceutical, and semiconductor industries. The high depth-to-width ratio allows for a single-pass weld on thicker wall pipes, which reduces welding time and cost. For example, a 6 mm thick stainless steel pipe can be welded in a single pass with A-TIG, whereas conventional TIG would require two or three passes. This is a significant productivity gain. The process is also used for welding of heat exchangers, pressure vessels, and other critical equipment.

Process Parameters and Flux Application

The application of the flux is critical. The flux is typically mixed with a solvent, such as acetone or alcohol, to form a paste. The paste is applied to the surface of the joint using a brush or a spray. The thickness of the flux layer should be about 0.1–0.2 mm. If the flux is too thick, it may cause slag inclusions or arc instability. If it is too thin, the effect is reduced. The flux must be applied uniformly, and it must be dry before welding.

Parameter Conventional TIG A-TIG with G1 A-T