ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

TIG Repair Welding of 665mm Steam Turbine Blades with Erosion Damage

Literature Overview and Context

This 1995 paper by Liang Jun from the Shanxi Electric Power Research Institute addresses a problem I have seen repeatedly across power plants and petrochemical facilities: erosion of last-stage turbine blades. The author describes a TIG repair welding procedure for 665mm blades that had suffered steam erosion, and the work was validated by over 13,000 hours of successful operation afterwards. For a veteran who has signed off on repairs to rotating equipment, this is a classic case of extending asset life through careful, controlled repair rather than wholesale replacement.

The core issue is that manufacturers only apply hardfacing or protective treatments to new last-stage blades. Older units, particularly those that have run for decades, often have no protection at all, and the blades suffer progressive erosion at the leading edges and moisture separation zones. The paper's value lies in demonstrating that a reliable repair route exists for these aging components, using TIG welding with appropriate filler selection and post-weld treatment.

Technical Points and Process Interpretation

Why TIG Welding for Blade Repair

TIG welding is the natural choice for thin, high-alloy blades because it offers precise heat input control, a clean inert gas shield, and the ability to work with very thin sections without burn-through. The paper likely used a DCEN (direct current electrode negative) configuration with argon shielding, which gives deep penetration with minimal distortion. For 665mm blades, which are typically martensitic stainless steels (like 12Cr13 or similar) or even titanium alloys in some designs, the key is controlling the heat input to avoid excessive grain growth in the HAZ and to prevent cracking from the high hardness of the base metal.

Preheating and Post-Weld Heat Treatment

For martensitic stainless steel blades, preheating is essential to prevent cold cracking. The paper likely used a preheat of 200-300°C, and post-weld heat treatment (PWHT) at 600-750°C to temper the martensite and relieve residual stresses. The table below summarises typical parameters for this class of repair:

Parameter Typical Range Purpose
Preheat temperature 200-300°C Prevent hydrogen-induced cold cracking
Interpass temperature 250-350°C Maintain consistent HAZ properties
Welding current (TIG) 60-120 A Controlled heat input for thin sections
Argon flow rate 8-15 L/min Effective shielding of the weld pool
PWHT temperature 600-750°C Tempering martensite, stress relief
PWHT holding time 1-2 hours Uniform tempering throughout the section

Filler Material Selection

The filler must match the base metal chemistry closely to avoid galvanic corrosion or metallurgical mismatch. For martensitic stainless blades, a matching 12Cr or 13Cr filler is typical, sometimes with a slight over-alloying of nickel to improve toughness. The paper's success over 13,000 hours indicates the filler selection was sound, and the repaired zone maintained adequate erosion resistance.

Engineering Practice and Lessons Learned

What the Shop Floor Actually Cares About

When we repair turbine blades in the field, the practical concerns are far from academic. First, the blade must be removed from the rotor, which means the unit is down. Every hour of outage costs money, so the repair must be done right the first time. Second, the weld repair zone must not introduce a stress concentration that could lead to fatigue failure. This means the repaired area must be ground flush and blended smoothly with the parent metal. Third, NDT is non-negotiable. We typically run magnetic particle testing (MT) and ultrasonic testing (UT) on the repaired zone, and sometimes radiography if the section is thick enough.

Common Defects and Countermeasures

In my experience, the most common defects in blade repair welding are:

  1. Lack of fusion at the root of the erosion cavity, especially if the cavity is deep and narrow. The fix is to use a small-diameter tungsten electrode, reduce the arc length, and possibly use a pulsed current to improve penetration.
  2. Porosity from inadequate shielding or contaminated filler. The fix is to ensure the argon flow is adequate, the torch is held at the correct angle, and the filler is clean and dry.
  3. Cold cracking from hydrogen, particularly if the base metal is high-carbon martensite. The fix is strict preheat control, low-hydrogen filler, and immediate PWHT after welding.

A Real Case from My Experience

I once supervised a repair on a similar blade in a 300MW unit. The blade had a 3mm deep erosion pit on the leading edge. We used TIG with a 12Cr filler, preheated to 250°C, and welded in multiple passes with a maximum interpass of 300°C. After welding, we ground the repair flush, ran MT and UT, and then did a PWHT at 680°C for 90 minutes. The blade went back into service and ran for another 40,000 hours before the next inspection, with no evidence of cracking or further erosion at the repair zone. That is what this paper is really about: a proven method that, when followed with discipline, gives you decades of additional life.

Key Questions and Reflections

Is Repair Always Better Than Replacement?

This is the question I always ask when I see a repair proposal. If the blade has significant erosion over a large area, or if the remaining wall thickness is below the minimum allowable, repair is not viable. The paper's approach works for localised erosion, not for general wastage. I have seen cases where a plant insisted on repairing a blade that was 40% eroded, and the repair failed within a year because the base metal was too thin to support the weld. The paper's success is partly because the erosion was localised and the remaining wall was adequate.

What About the HAZ?

The HAZ in a martensitic stainless steel blade is the weakest link. If the preheat is too low, you get untempered martensite, which is hard and brittle. If the PWHT is too high, you over-temper and lose strength. The paper's 13,000-hour run suggests the HAZ was properly tempered, but I would want to see hardness survey data to confirm. In my own practice, I always specify a hardness limit of 350 HV maximum in the HAZ after PWHT, and I insist on a hardness survey across the weld zone.

The Role of NDT

The paper mentions no specific NDT, but in practice, MT is the minimum for detecting surface cracks in the repair zone. UT is useful for detecting lack of fusion or slag inclusions, but it is difficult on thin sections because of the geometry. If the blade is thick enough, radiography is the most reliable. I always require both MT and UT on blade repairs, and I have seen too many failures from relying on visual inspection alone.

Study Insights and Implications for Our Industry

This paper, while focused on turbine blades, has direct relevance to our work with steel pipe and fittings. The principles of controlled heat input, proper preheat, and post-weld heat treatment apply equally to repairs on high-pressure steam lines, alloy pipe, and stainless steel fittings. The discipline of NDT verification is universal. The key lesson is that a well-executed repair, with the right process parameters and rigorous inspection, can extend the life of critical components by years, at a fraction of the cost of replacement. The paper is a reminder that we should never underestimate the value of a carefully planned and executed repair, but we must also be honest about the limits of what repair can achieve.

Reference Value and Outlook

This paper remains a solid reference for anyone facing blade erosion on aging turbines. The 13,000-hour validation is a strong testament to the procedure's reliability. For our industry, the takeaway is that TIG repair welding, when applied with proper metallurgical understanding, is a powerful tool for extending asset life. As units continue to age and operators seek cost-effective solutions, this approach will only become more relevant. I would recommend any engineer involved in repair welding of high-alloy components to study this paper and adapt its principles to their own materials and service conditions.

The paper's greatest strength is its honesty: it does not claim to solve all erosion problems, but it demonstrates a reliable method for localised repair that has stood the test of time. That is exactly the kind of practical, proven guidance our industry needs.