ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Argon Arc Welding Process for Copper-Titanium Bimetallic Composite Pipes

Introduction and Literature Overview

The paper by Wang Yongfang, Wang Ge, Zhang Yanfei, and Guo Chongxiao, published in Hot Working Technology in 2011, addresses a challenging and highly specialized topic: the welding of copper-titanium bimetallic composite pipes. These pipes are used in applications where the excellent corrosion resistance of titanium is combined with the high thermal and electrical conductivity of copper. Common applications include heat exchangers, marine structures, and chemical processing equipment, where the outer titanium layer provides corrosion protection and the inner copper layer ensures efficient heat transfer.

The authors analyze the weldability of copper-titanium composite pipes and propose a unique groove design and argon arc welding process. They use a silver-based brazing filler metal (BAg72Cu) as a transition material and employ a three-step welding process: "TIG root pass + TIG brazing transition + TIG cap pass." The welded joints are evaluated using X-ray radiography, chemical composition analysis, tensile testing, bending testing, metallographic examination, microhardness testing, and electrochemical corrosion testing. The results demonstrate that the proposed process produces joints with ideal chemical composition, microstructure, mechanical properties, and corrosion resistance.

Weldability Analysis of Copper-Titanium Composite Pipes

The weldability of copper-titanium composite pipes is inherently difficult due to the significant differences in the physical and metallurgical properties of the two metals.

Property Copper Titanium Implication for Welding
Melting Point (°C) 1083 1668 Titanium requires higher heat input
Thermal Conductivity (W/m·K) 400 21.9 Copper dissipates heat rapidly, making fusion difficult
Coefficient of Thermal Expansion (10⁻⁶/K) 17.0 8.6 Differential expansion causes residual stress
Reactivity with Oxygen Low High Titanium oxidizes readily, requiring excellent shielding
Solubility of Interstitial Elements Low High Titanium embrittles with O, N, H

The most critical issue is the formation of brittle intermetallic compounds, such as TiCu, Ti₂Cu, and Ti₃Cu₄, when copper and titanium are melted together. These compounds have poor mechanical properties and are highly susceptible to cracking. Therefore, direct fusion welding of copper to titanium is not feasible. The authors correctly identify this problem and propose a solution that avoids direct melting of the two metals.

Another challenge is the high thermal conductivity of copper, which makes it difficult to achieve fusion at the root of the joint. The heat is rapidly conducted away from the weld pool, leading to lack of fusion and poor penetration. The authors address this by using a unique groove design that concentrates the heat and by employing a high-energy welding process (TIG) with careful control of the heat input.

Proposed Groove Design and Welding Process

The authors propose a unique groove design that is specifically tailored to the copper-titanium composite pipe. The groove is designed to allow the use of a silver-based brazing filler metal (BAg72Cu) as a transition material, which has a melting point lower than both copper and titanium. The brazing filler metal wets both surfaces and forms a joint without melting the base metals, thereby avoiding the formation of brittle intermetallic compounds.

The welding process consists of three steps:

  1. TIG root pass: The root pass is performed using a TIG welding process with a suitable filler metal to ensure complete fusion of the copper inner layer. The root pass provides a sound base for the subsequent brazing and cap passes.
  2. TIG brazing transition: The transition pass is performed using the silver-based brazing filler metal (BAg72Cu). The brazing filler metal is applied to the joint area, and the heat from the TIG arc melts the filler metal, which wets the titanium and copper surfaces. The brazing filler metal does not melt the base metals, but forms a metallurgical bond with both.
  3. TIG cap pass: The cap pass is performed using a TIG welding process with a suitable filler metal to provide a smooth and sound weld surface. The cap pass ensures that the joint has adequate reinforcement and that the brazed transition is protected from the environment.
Step Process Filler Metal Purpose
1 TIG root pass Cu-based filler Fusion of copper inner layer
2 TIG brazing transition BAg72Cu Metallurgical bond between Cu and Ti
3 TIG cap pass Ti-based filler Smooth and sound weld surface

This three-step process is a clever and practical solution to a difficult welding problem. By using a brazing filler metal as a transition, the authors avoid the formation of brittle intermetallic compounds while achieving a strong and corrosion-resistant joint.

Joint Performance Evaluation

The authors conducted a comprehensive evaluation of the welded joints, including X-ray radiography, chemical composition analysis, tensile testing, bending testing, metallographic examination, microhardness testing, and electrochemical corrosion testing.

Test Method Result Assessment
X-ray Radiography No defects detected Sound joint
Chemical Composition Brazing layer rich in Ag and Cu Confirms brazing filler metal present
Tensile Strength Meets or exceeds base metal Strong joint
Bending Test No cracks after bending Good ductility
Metallographic Examination No intermetallic compounds at interface Good metallurgical bond
Micro