Three-Dimensional FEM Simulation of Wall Thickness Variation in Hot Continuous Rolling of Steel Pipes
Introduction to the Process
The hot continuous rolling of seamless steel pipes is a complex, multi-stage process that involves a series of rolling stands, each with a pair of grooved rolls, operating on a mandrel that is either held stationary or moves with the pipe. The process is used to produce high-quality seamless pipes with tight dimensional tolerances, and it is particularly critical for applications such as oil country tubular goods (OCTG), line pipe, and boiler tubes. The paper by Zhao Zhiyi and colleagues from the University of Science and Technology Beijing and Baosteel addresses a fundamental question: how does the wall thickness evolve through the rolling stands, and what is the role of the mandrel force in the process? The authors used a three-dimensional finite element model to simulate the eight-stand continuous rolling of a 20-grade steel pipe with dimensions of 119.0 mm outer diameter and 9.25 mm wall thickness, on a floating mandrel.
Simulation Setup and Methodology
The finite element model was built to represent the full eight-stand rolling process, including the rolls, the mandrel, and the pipe. The rolls were modeled as rigid bodies with the appropriate groove geometry, while the pipe was modeled as a deformable body with elastic-plastic material properties. The mandrel was modeled as a rigid body that moves with the pipe at a controlled speed, representing the floating mandrel condition.
| Parameter | Value |
|---|---|
| Pipe material | 20-grade steel (0.20% C) |
| Initial outer diameter | 119.0 mm |
| Initial wall thickness | 9.25 mm |
| Number of stands | 8 |
| Mandrel type | Floating mandrel |
| Rolling temperature | Approximately 1000-1100 °C |
| Simulation type | 3D elastic-plastic finite element |
The model output included the equivalent plastic strain at each stand exit, the wall thickness distribution, the roll force, and the mandrel force. These results were then compared with measured data from an actual rolling campaign at Baosteel.
Key Findings on Wall Thickness Evolution
The simulation revealed a clear pattern in the wall thickness reduction across the eight stands. The majority of the reduction occurs in the first six stands, with the seventh and eighth stands contributing very little to further wall thinning. This is an important finding because it indicates that the final stands are primarily used for sizing and shaping, not for significant deformation.
| Stand Number | Wall Thickness Reduction (%) | Outer Diameter Reduction (%) | Equivalent Plastic Strain |
|---|---|---|---|
| 1 | 18.5 | 12.3 | 0.35 |
| 2 | 22.1 | 15.6 | 0.52 |
| 3 | 19.8 | 14.2 | 0.68 |
| 4 | 15.2 | 11.8 | 0.79 |
| 5 | 10.4 | 8.5 | 0.86 |
| 6 | 6.8 | 5.2 | 0.91 |
| 7 | 2.1 | 1.8 | 0.93 |
| 8 | 0.8 | 0.6 | 0.94 |
The final wall thickness was found to be uniform around the circumference, and the pipe cross-section was round and free from significant ovality. This is a critical quality indicator, as wall thickness variation can lead to premature failure in service, particularly in high-pressure applications.
Analysis of Roll Force and Mandrel Force
The simulation also provided insights into the force distribution during the rolling process. The roll force was found to decrease progressively from the first stand to the eighth stand, reflecting the decreasing reduction in cross-sectional area. The mandrel force, however, was found to be consistently higher than the roll force at each stand. This is a significant finding because it indicates that the mandrel is subjected to a substantial axial load, which can cause wear, deformation, and even fracture if not properly managed.
| Stand Number | Roll Force (kN) | Mandrel Force (kN) |
|---|---|---|
| 1 | 1850 | 2100 |
| 2 | 1620 | 1950 |
| 3 | 1380 | 1720 |
| 4 | 1150 | 1480 |
| 5 | 890 | 1210 |
| 6 | 620 | 890 |
| 7 | 310 | 520 |
| 8 | 120 | 240 |
The high mandrel force also means that the inner surface of the pipe experiences significant plastic strain and frictional heating. This can lead to surface defects such as laps, folds, and internal cracks if the mandrel surface is not properly lubricated. The authors recommend that the mandrel be coated with a suitable lubricant, such as a glass-based or graphite-based lubricant, to reduce friction and prevent surface damage.
Practical Implications for the Shop Floor
The findings from this simulation have direct implications for the production of seamless steel pipes.
- The rolling schedule should be designed so that the majority of the wall reduction occurs in the early stands. This ensures that the material is still at a high temperature and has sufficient ductility to accommodate the deformation without cracking.
- The final stands should be used primarily for sizing and roundness correction. Excessive reduction in the final stands can lead to residual stresses and poor surface quality.
- The mandrel force is a critical process parameter. It should be monitored continuously, and any sudden increase may indicate a lubrication failure or a change in the material properties.
- Proper lubrication of the mandrel is essential. The lubricant must be applied uniformly and must be able to withstand the high temperatures and pressures encountered in the rolling process.
- The wall thickness uniformity achieved in the simulation is a good indicator of process stability. If the actual wall thickness variation exceeds the specified tolerance, the rolling schedule should be reviewed.
Comparison with Measured Data
The authors compared the simulated wall thickness, outer diameter, and roll force with measured data from the actual rolling process. The agreement was excellent, with deviations of less than 5% for all parameters. This validates the finite element model and confirms that it can be used as a predictive tool for process design and optimization. For a plant engineer, this is a valuable capability, as it allows for the evaluation of new rolling schedules without the need for expensive and time-consuming trial runs.
Conclusion
The paper by Zhao Zhiyi and colleagues provides a comprehensive analysis of the wall thickness evolution and force distribution in the hot continuous rolling of seamless steel pipes. The key findings, that the majority of the reduction occurs in the first six stands and that the mandrel force exceeds the roll force, have direct implications for process design and operation. The validated finite element model can be used to optimize rolling schedules, reduce defects, and improve product quality. For anyone involved in the production of seamless pipes, this paper is a valuable reference that bridges the gap between academic research and industrial practice. The insights gained from this simulation have been applied in our own plants to refine rolling schedules and improve mandrel lubrication, resulting in better surface quality and tighter dimensional tolerances.
Zhuojin Pipe Fitting Co., Ltd