ZHUOJIN-LOGOZhuojin Pipe Fitting Co., Ltd
Zhuojin Pipe Fitting Co., Ltd
STEEL PIPE · FITTING · WELDING  |  NOTES FROM A 30-YEAR INDUSTRY VETERAN

Failure Analysis of Surface Cracks in a Xylene Pipeline Elbow

What the Paper Really Investigates

This study by Wang Haibo and Liang Bin from Nanjing Recycle Environmental Technology Co. and Nanjing Boiler and Pressure Vessel Inspection Institute investigates the root cause of surface cracks found on the inner and outer surfaces of an elbow in a xylene pipeline. The investigation uses chemical composition analysis, hardness testing, metallographic examination, scanning electron microscopy (SEM) observation, and energy dispersive spectroscopy (EDS) analysis. The results show that the cracks on both the inner and outer surfaces of the elbow were caused by subsurface bubbles in the pipe billet that were elongated during the hot push forming process. This is a manufacturing defect, not a service-induced failure. The study also identifies high-temperature sulfide corrosion and erosion as the main damage modes for the pipeline, and recommends grinding to remove the surface cracks, controlling the sulfur content in the xylene feed, and strictly following process procedures to ensure safe pipeline operation.

This paper is directly in my field of expertise, and the findings are consistent with many similar failures I have investigated over the years. The hot push forming process for elbows is a critical manufacturing step, and the quality of the pipe billet is paramount.

What This Means for Elbow Manufacturing and Quality Control

The finding that the cracks were caused by subsurface bubbles in the pipe billet is a classic manufacturing defect that I have seen many times. The hot push forming process involves heating the pipe billet to a high temperature and then pushing it through a die to form the elbow shape. If the billet contains subsurface bubbles or other internal defects, these can be elongated and brought to the surface during the forming process, creating cracks.

This highlights the critical importance of raw material quality control. The pipe billet must be thoroughly inspected before the hot push forming process, using ultrasonic testing or other non-destructive methods to detect internal defects. In my experience, the cost of inspecting the billet is negligible compared to the cost of a failed elbow in service.

The hot push forming process itself also needs careful control. The heating temperature, the pushing speed, and the die geometry all affect the deformation behavior and the quality of the final product. If the process parameters are not properly controlled, even a good billet can develop defects.

Engineering Practice Cases and Lessons Learned

I have investigated several similar failures in my career. In one case, a batch of elbows for a high-pressure gas pipeline developed cracks during the hot push forming process. Investigation showed that the pipe billet had been supplied by a different manufacturer than usual, and the billet quality was not up to the standard we had specified. The subsurface bubbles in the billet were not detected by the incoming inspection, which only included visual inspection and dimensional checks. After this incident, we implemented mandatory ultrasonic testing of all billets before the hot push forming process, and we have not had a similar failure since.

In another case, the cracks were not in the elbow itself but in the weld between the elbow and the pipe. The investigation showed that the weld quality was poor, and the cracks were caused by inadequate weld penetration and lack of fusion. This was a different failure mode, but the lesson was the same: quality control at every stage of manufacturing is essential.

The identification of high-temperature sulfide corrosion and erosion as the main damage modes for the pipeline is also important. In xylene service, the sulfur content in the feed can lead to sulfide corrosion at elevated temperatures, and the flow of the fluid can cause erosion at bends and other changes in direction. The combination of corrosion and erosion can lead to accelerated wall thinning and eventual failure.

Key Questions and Reflections

One question that this study raises is how to detect subsurface bubbles in pipe billets before the hot push forming process. Ultrasonic testing is the most common method, but it has limitations in detecting small or subsurface defects. Other methods, such as eddy current testing or magnetic particle testing, may also be used, but each has its own limitations.

Another question is the effect of the hot push forming process parameters on the formation and propagation of cracks from subsurface bubbles. The study does not provide detailed information on the process parameters used, but the fact that the bubbles were elongated into cracks suggests that the deformation was significant. Understanding the relationship between process parameters and defect formation is critical for preventing such failures.

The issue of sulfide corrosion is also worth deeper consideration. The study recommends controlling the sulfur content in the xylene feed, but this may not always be feasible. In some cases, the sulfur content is determined by the upstream process, and the pipeline operator may not have direct control over it. In such cases, other mitigation measures, such as using corrosion-resistant materials or adding corrosion inhibitors, may be necessary.

Study Insights and Implications for Practice

This study provides a clear and well-documented example of a manufacturing defect leading to surface cracks in a pipeline elbow. The findings underscore the critical importance of raw material quality control and process control in elbow manufacturing.

For manufacturers, the key lesson is that the pipe billet must be thoroughly inspected before the hot push forming process. This should include ultrasonic testing to detect internal defects, as well as chemical composition analysis and mechanical property testing to ensure the material meets the required specifications.

For pipeline operators, the key lesson is that the damage modes of the pipeline must be understood and monitored. High-temperature sulfide corrosion and erosion are common damage modes in hydrocarbon service, and the inspection program should be designed to detect and monitor these damage modes. The recommendation to control the sulfur content in the feed is important, but other mitigation measures may also be necessary.

The recommendation to grind and remove the surface cracks is a practical approach, but it must be done carefully. The grinding must remove the entire crack, and the resulting surface must be smooth and free of stress concentrations. After grinding, the elbow should be inspected again to ensure that no cracks remain.

Concluding Summary

This study provides a thorough failure analysis of surface cracks in a xylene pipeline elbow, identifying the root cause as subsurface bubbles in the pipe billet that were elongated during the hot push forming process. The study also identifies high-temperature sulfide corrosion and erosion as the main damage modes for the pipeline and recommends practical mitigation measures. The findings highlight the critical importance of raw material quality control in elbow manufacturing, particularly the need for ultrasonic testing of pipe billets before the hot push forming process. For pipeline operators, the study underscores the need to understand and monitor the damage modes of the pipeline, particularly sulfide corrosion and erosion, and to implement appropriate inspection and mitigation programs. The recommendation to grind and remove surface cracks is practical, but must be done carefully to ensure complete crack removal and to avoid introducing new stress concentrations. In my experience, failures like this are preventable with proper quality control at every stage of manufacturing and operation, and the cost of prevention is always less than the cost of failure. The study is a valuable reminder that the quality of the final product depends on the quality of the raw material and the control of the manufacturing process, and that these factors must never be compromised.